Diamond-Point Spade Bits: A Thinned, Wide-Angled Point Does More of the Cutting (Southall, 1975)
Forge

Created by

Forge

13. November 2026NO
0
0
0
0
0

Diamond-Point Spade Bits: A Thinned, Wide-Angled Point Does More of the Cutting (Southall, 1975)

William Southall of Moonah, Australia, invented this spade bit. US 3,920,350, dated 18 November 1975 and assigned to The Stanley Works, was granted after his death. The point is diamond-shaped in section. It flares out slightly where it leaves the blade, then closes at a large angle, and its faces are ground thinner towards the tip. So it cuts more and the blade's edges less. The cutting edges lean forward towards the outside and are bevelled opposite ways. The corners at the root of the point are undercut, because sharp corners there cut poorly. His figures are for a one-inch bit; we forge 5/8, 3/4 and 1 inch bits with his point and angles.
Intermediate
About 1 day

Instructions

1

His one-inch figures

Loading Jupyter Notebook...
2

Read US 3,920,350

"As a result of the fact that the point 16 is provided with a relatively large point angle, the point 16 is caused to perform more of the cutting function as compared to that performed by the cutting surfaces 42 and 44 of the blade 14."
3

Forge the blades

Cut three 170 mm lengths of 10 mm octagonal tool steel. Heat 50 mm of one end to a bright orange in the forge and flatten it on the anvil to about 3 mm thick, centred on the bar. Hammer across it with the peen to spread it wider than the bit, about 2 mm over its size: 18, 22 and 27 mm. Draw the neck down smoothly where the blade meets the bar and keep the blade in line with it. Reheat as soon as the colour fades to red. Finally heat each one to a cherry red and let it cool slowly in the air, to soften it for filing.

Materials for this step:

Octagonal Tool Steel BarOctagonal Tool Steel Bar3 pieces

Tools needed:

HacksawHacksaw
Bench ViseBench Vise
ForgeForge
AnvilAnvil
Forge HammerForge Hammer
Forge TongsForge Tongs
Welding GlovesWelding Gloves
Safety GlassesSafety Glasses
4

Print the grinding template

Full-size A4 template: the outlines of the 5/8, 3/4 and 1 inch bits with Southall's point, forward-leaning cutting edges and tapered sides, and the hanging hole. Print at 100 %; its 50 mm bar must measure 50 mm.
Design FilePDFCC0 - Free
5

Grind the outline

Glue each bit's outline from the template on its blade, centred on the bar. Grind to the lines on the bench grinder, dipping the steel in water often: the two sides parallel, the shoulders square across, the point in the middle. Grind the blade's two faces flat and parallel to 2.5 mm. Grind three flats on the end of the shank, a third of the way round from each other, 20 mm long, for the chuck's jaws. Drill a 3 mm hole through the blade at the template's circle.

Tools needed:

Inkjet PrinterInkjet Printer
GlueGlue
Bench GrinderBench Grinder
Quench BucketQuench Bucket
WaterWater
File SetFile Set
Bench ViseBench Vise
Digital Caliper 6-InchDigital Caliper 6-Inch
Safety GlassesSafety Glasses
6

Grind Southall's bevels and point

Bevel each side of the blade about 2 degrees, one side from the top face and the other from the bottom face. Bevel the two cutting edges about 10 degrees behind the edge, again opposite ways, so each cuts as the bit turns. Bevel the point's converging edges about 10 degrees the same opposite ways, giving the point its diamond section. Grind the point's top and bottom faces thinner towards the tip until they meet there at about 8 degrees. Round the two corners where the point meets the cutting edges with the edge of a needle file.

Tools needed:

Bench GrinderBench Grinder
Quench BucketQuench Bucket
WaterWater
Needle File SetNeedle File Set
Bench ViseBench Vise
Digital Caliper 6-InchDigital Caliper 6-Inch
7

Harden and temper

Heat the blade and the neck evenly to a cherry red, until a magnet no longer sticks to it, and quench it straight down in water, moving it up and down. Rub the faces bright with a stone. Heat the shank gently 30 mm behind the blade and watch the colours run down; quench again as soon as a dark straw colour reaches the shoulders and the point. Do the other two.

Tools needed:

ForgeForge
Forge TongsForge Tongs
Small MagnetSmall Magnet
Quench BucketQuench Bucket
WaterWater
Sharpening StoneSharpening Stone
Welding GlovesWelding Gloves
Safety GlassesSafety Glasses
8

Sharpen and test

Hone the cutting edges on the shoulders and the point with the stone, keeping their angles, and take the burr off. Chuck a bit by its flats and bore a scrap of hardwood: it should start on the point without wandering, cut two clean shavings from the shoulders and leave a round hole of its own size; check it with the caliper.

Tools needed:

Sharpening StoneSharpening Stone
Cordless DrillCordless Drill
Hardwood BoardHardwood Board
Digital Caliper 6-InchDigital Caliper 6-Inch
Safety GlassesSafety Glasses
9

Troubleshooting

Spade bit troubleshooting.

Flow

Loading...
10

History and honest limits

**William Southall**, deceased, late of Moonah, Australia, by Dorothy I. Southall, administratrix, assignor to The Stanley Works, US 3,920,350, dated 18 November 1975, filed 11 February 1974. He claimed a point "having side edges diverging towards said side edges of said blade and a pair of faces converging to the tip", giving "a generally rhomboidal transverse cross section", with the blade's leading edges inclined towards the point and at opposite angles. His figures are for a one-inch bit and are approximate; we use his point and angles on all three sizes. His shank is round with a hexagonal end; ours is octagonal tool steel with three ground flats. He gives no heat treatment; the hardening is our house practice.

Materials

1

Tools Required

20

Design Files

1

Related Blueprints

These blueprints share knowledge with this one โ€” techniques, materials, or principles that connect them in the learning graph.

CC0 Public Domain

This blueprint is released under CC0. You are free to copy, modify, distribute, and use this work for any purpose, without asking permission.

Support the Maker by purchasing products through their Blueprint where they earn a Maker Commission set by Vendors, or create a new iteration of this Blueprint and include it as a connection in your own Blueprint to share revenue.

Discussion

(0)

Log in to join the discussion

Loading comments...