Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1260 °C (Went, Philips 1956, Ex. 28)
Charlie

Tạo bởi

Charlie

28. tháng Mười 2026DE
1
0
0
0
0

Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1260 °C (Went, Philips 1956, Ex. 28)

A ceramic magnet with both barium and strontium: 0.5 mol barium carbonate and 0.5 mol strontium carbonate to 3 mol iron oxide, milled 15 hours, pressed and passed through a 1260 °C furnace in 20 minutes. Went's rod held 1,665 gauss with a coercive force of 3,235 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 28. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Nâng cao
2 days

Hướng dẫn

1

Weigh the carbonates and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol), 73.8 g strontium carbonate (0.5 mol), 483.3 g ferric oxide (3 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Vật liệu cho bước này:

Bari cacbonat (witherit)Bari cacbonat (witherit)99.2 g
Stronti cacbonatStronti cacbonat73.8 g
Oxit sắt(III)Oxit sắt(III)483.3 g

Công cụ cần thiết:

Cân hai đĩaCân hai đĩa
Găng tay cao suGăng tay cao su
Mặt nạ phòng độc P100Mặt nạ phòng độc P100
2

Mill with alcohol 15 hours, dry

Grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

Công cụ cần thiết:

Máy nghiền bi sắtMáy nghiền bi sắt
Etanol phẩm cấp thí nghiệm, 95 %Etanol phẩm cấp thí nghiệm, 95 %
Lò sấyLò sấy
3

Press the powder

Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.

Công cụ cần thiết:

Máy ép thủy lựcMáy ép thủy lực
Khuôn ép đĩaKhuôn ép đĩa
4

Pass through a 1260 °C zone in 20 minutes

Sinter at 1260 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.

Công cụ cần thiết:

Lò ốngLò ống
Găng tay chịu nhiệtGăng tay chịu nhiệt
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Công cụ cần thiết:

Nam châm điệnNam châm điện
La bànLa bàn

Vật liệu

3

Công cụ yêu cầu

12

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...