Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper
Bromide paper is paper coated with silver bromide in gelatin, the printing and enlarging paper of the darkroom. Thorpe (1913) gives a beginner's emulsion: gelatin swelled in potassium bromide solution, silver nitrate made clear with strong ammonia, the two joined under ruby light, ripened, set, washed, and spread on paper as on a glass plate. From the moment the silver goes in, work only by ruby light. Grain and ounce figures are Thorpe's; the gram conversions and the 10-sheet batch are ours.
The picture: our own drawing.
Nâng cao
4 days
Hướng dẫn
1
1
Swell the gelatin
Swell the gelatin
Dissolve 185 grains (12.0 g) of potassium bromide in 5 oz (142 ml) of water. Cover 300 grains (19.4 g) of hard gelatin with it and stir until it softens and swells.
Vật liệu cho bước này:
Kali bromua12 g
Bột gelatin19.4 gCông cụ cần thiết:
Nước
Cốc thủy tinh (becher)
Đũa khuấy thuỷ tinh
Cân hai đĩa2
2
Dissolve the silver
Dissolve the silver
Dissolve 231 grains (15.0 g) of silver nitrate in 5 oz (142 ml) of water with gentle heat in the water bath. Add strong ammonia (0.880) a little at a time, stirring, until the precipitate that first forms dissolves again.
Vật liệu cho bước này:
Bạc nitrat15 gCông cụ cần thiết:
Nước
Dung dịch amoniac đặc (0.880)
Cốc thủy tinh (becher)
Đũa khuấy thuỷ tinh
Nồi lớn (đáy, dùng cho nồi cách thủy)3
3
Melt the gelatin, never above 35 °C
Melt the gelatin, never above 35 °C
Stand both vessels in the pan of water, never above 35 °C, stirring, until the gelatin is perfectly liquid. Up to here ordinary light is fine.
Công cụ cần thiết:
Nồi lớn (đáy, dùng cho nồi cách thủy)
Nhiệt kế
Đũa khuấy thuỷ tinh4
4
Add the silver under ruby light
Add the silver under ruby light
From now on, ruby light only. Pour the silver solution into the gelatin in a thin stream, stirring all the time. Rinse the silver beaker with about 1 oz (28 ml) of warm water into the emulsion.
Công cụ cần thiết:
Đèn an toàn đỏ ruby
Cốc thủy tinh (becher)
Đũa khuấy thuỷ tinh
Nước5
5
Ripen
Ripen
Leave the emulsion in the hot water for half to three-quarters of an hour.
Công cụ cần thiết:
Nồi lớn (đáy, dùng cho nồi cách thủy)
Đèn an toàn đỏ ruby6
6
Set in the dark
Set in the dark
Pour it into a flat dish, put it in a light-tight box and let it set for at least 24 hours; two or three days is better.
Công cụ cần thiết:
Khay gốm nông
Hộp kín sáng7
7
Wash through canvas
Wash through canvas
Scrape the set jelly onto wet coarse canvas and tie it into a bag. Knead it under water so it squeezes through in threads. Pour off the water, cover with fresh, wait 5 minutes and pour off: six to eight times.
Công cụ cần thiết:
Xẻng lật
Vải bạt
Dây
Nước
Đèn an toàn đỏ ruby8
8
Drain and store
Drain and store
Turn the threads onto a strainer covered with a cloth and let the water drain. Rinse with methylated spirit and keep in a lidded jar until coating.
Công cụ cần thiết:
Rây lọc
Vải mút-xơ-lin
Cồn công nghiệp
Lọ thủy tinh có nắp
Đèn an toàn đỏ ruby9
9
Coat the paper
Coat the paper
Melt the emulsion in the warm water bath. Lay a sheet of paper flat on a levelled glass slab. Pour emulsion on the middle to cover nearly half the sheet, and spread it to each end with a glass rod 2 inches wider than the sheet, held just off the surface.
Vật liệu cho bước này:
Giấy10 tờCông cụ cần thiết:
Nồi lớn (đáy, dùng cho nồi cách thủy)
Tấm kính
Thước thủy (nivô)
Đũa khuấy thuỷ tinh
Đèn an toàn đỏ ruby10
10
Dry
Dry
When the coat has set, move the sheets to a rack in a drying box with a current of air. They dry in 12 to 48 hours. Keep them in the light-tight box.
Công cụ cần thiết:
Giá phơi
Hộp kín sángVật liệu
4- 12 gTạm thời
- 19.4 gTạm thời
- 15 gTạm thời
- 10 tờTạm thời
Công cụ yêu cầu
20- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.