Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)
Youblob · CC0
Charlie

Tạo bởi

Charlie

27. tháng Mười 2026DE
7
0
0
0
0

Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)

A trace of hot potash opens the ring of D4 and strings it into a long, thick chain. Water added a little at a time then cuts the chains back and leaves hydroxyl groups on their ends, which is what later lets the oil cure into rubber. This is Louis Ceyzeriat's oil A, the base of every sealant in his patent: 21,000 centistokes, 0.15 % hydroxyl. Source: L. Ceyzeriat (Rhône-Poulenc), US 3,133,891 (1964), column 4. His neutraliser was the precipitated silica Hi-Sil X303; we use our precipitated silica in its place. The potash mix and the equipment are ours. Picture drawn by Youblob.
Nâng cao
2 days

Hướng dẫn

1

Make the 10 % potash

Dissolve 0.5 part of potassium hydroxide in 4.5 parts of water (our arithmetic for 5 parts of a 10 % solution). All parts are by weight.

Vật liệu cho bước này:

Kali hydroxitKali hydroxit0.5 parts
NướcNước4.5 parts

Công cụ cần thiết:

Bình thủy tinhBình thủy tinh
Cân hai đĩaCân hai đĩa
2

Heat D4 with the potash under nitrogen

Heat 5000 parts of octamethylcyclotetrasiloxane (it melts at 17.5 °C) with the 5 parts of 10 % potash at 150 °C for 3½ hours under nitrogen. The oil thickens to 31,000 centistokes while hot.

Vật liệu cho bước này:

Octametylxiclotetrasiloxan (D4)Octametylxiclotetrasiloxan (D4)5000 parts

Công cụ cần thiết:

Bình cầu chưng cất thủy tinhBình cầu chưng cất thủy tinh
Bếp điện phẳngBếp điện phẳng
Nhiệt kếNhiệt kế
Que khuấyQue khuấy
Bình khí nitơBình khí nitơ
3

Add water a little at a time

Still hot, add 16.5 parts of water in small portions over 3 hours 40 minutes. The hot oil thins to 1730 centistokes.

Vật liệu cho bước này:

NướcNước16.5 parts

Công cụ cần thiết:

Bình cầu chưng cất thủy tinhBình cầu chưng cất thủy tinh
Bếp điện phẳngBếp điện phẳng
Nhiệt kếNhiệt kế
Que khuấyQue khuấy
4

Cool, then neutralise with silica

Let it cool for 15 hours. Then stir in 50 parts of precipitated silica to neutralise the potash. The liquid now measures 13,400 centistokes at 25 °C.

Vật liệu cho bước này:

Silica kết tủaSilica kết tủa50 parts

Công cụ cần thiết:

Bình cầu chưng cất thủy tinhBình cầu chưng cất thủy tinh
Que khuấyQue khuấy
5

Strip the volatiles at 195–200 °C

Heat it to about 195–200 °C in a current of nitrogen, with a water condenser on the outlet. 655 parts of liquid distil over; 4345 parts of oil A stay in the boiler, 21,000 centistokes at 25 °C with 0.15 % hydroxyl groups.

Công cụ cần thiết:

Bình cầu chưng cất thủy tinhBình cầu chưng cất thủy tinh
Dàn ống ngưng tụDàn ống ngưng tụ
Bếp điện phẳngBếp điện phẳng
Nhiệt kếNhiệt kế
Bình khí nitơBình khí nitơ
Lọ thủy tinh có nắpLọ thủy tinh có nắp

Vật liệu

4

Công cụ yêu cầu

9

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...