Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)
Forge

Tạo bởi

Forge

1. tháng Mười Một 2026NO
3
0
0
0
0

Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)

The renowned bar iron of Dannemora was refined in the old Walloon way: long white pigs melt drop by drop before a cold blast in a small, very hot charcoal hearth, the finer works the metal with an iron staff until it comes to nature, and the lump is drawn out under water-driven hammers. Result: bars 12 ft long of about 60 lb; 6 tons a week from one hearth, 80 % of the weight of the pig. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 599-601, after Tunner and A. Grill. Picture drawn by Youblob.
Chuyên gia
about 30 minutes per lump; 8-hour shifts

Hướng dẫn

1

Build the finery hearth

Make the hearth of cast-iron plates: a 2-inch bottom plate on about 3 inches of pounded slag, over a cast-iron box with channels to drain water. From the tuyere it is 10-11½ inches to the back-plate, 22-24 inches to the work-plate and 22-24 inches to the opposite side. Depth: 7-8 inches under the tuyere, 14-15 under the back-plate, 15-18 opposite the tuyere. No tapping hole: the slag is never let out.

Công cụ cần thiết:

Lò luyện sắtLò luyện sắt
2

Set the tuyere and blast

The tuyere nozzle is semicircular, flat side down, 20-25 lines broad and 16-17 lines high, and projects 3½ inches; the blast-pipe nozzle sits 4 inches back inside it. Use cold blast. The blowing machine is not described.

Công cụ cần thiết:

Lò luyện sắtLò luyện sắt
Bễ thổiBễ thổi
3

Lay in the pigs

Use white or strongly mottled pig in long pigs about 9 inches broad, 15-18 feet long, 3-4 inches thick at one end and 1-2 at the other. Lay them across the back-plate, one end sloping down over the tuyere, usually two one above the other, and push them forward as the ends melt.

Vật liệu cho bước này:

Gang trắng than củiGang trắng than củi1 long pigs

Công cụ cần thiết:

Lò luyện sắtLò luyện sắt
4

Light and make the slag bath

Fill the front of the hearth with moistened small charcoal and the rest with charcoal, light it and turn on the blast. To make enough slag bath, melt down some large finery scraps or, failing these, several shovelfuls of hammer scale.

Công cụ cần thiết:

Than củi - nghiền mịnThan củi - nghiền mịn
NướcNước
Than củiThan củi
Vảy sắt rènVảy sắt rèn
XẻngXẻng
5

Reheat the last bloom

At the start of each heat, hold the bloom from the last lump with tongs, as steeply as you can, in the front of the hearth to reheat it for drawing out.

Công cụ cần thiết:

Kìm rènKìm rèn
6

Work the metal with the staff

As soon as the first pig iron melts, work it with an iron staff: bring the metal on the tuyere side up from the bottom towards the middle into the blast, once to the left and once to the right of the reheating bloom. About 70 lb melts in 20 minutes; thin pieces of malleable iron then cling to the staff.

Công cụ cần thiết:

Que sắt trònQue sắt tròn
7

Form the lump

Stop the flow of fresh molten pig, break up all the metal above the tuyere, melt it down and gather it into a lump about 12 by 15 inches. One lump takes 28 minutes on average (25-30).

Công cụ cần thiết:

Que sắt trònQue sắt tròn
Kìm rènKìm rèn
8

Draw out the bar

Heat each lump 6-8 times in a separate fire and draw it out under water-driven hammers into a bar 12 feet long of about 60 lb. One finery, one drawing-out forge and one hammer make 6 tons of bars a week; the bars weigh 80 % of the pig, and take 3 tons of charcoal per ton.

Công cụ cần thiết:

Lò rènLò rèn
Búa rèn camBúa rèn cam
Guồng nướcGuồng nước
Kìm rènKìm rèn

Vật liệu

1

Công cụ yêu cầu

12

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...