Arthur F. Payne · Public domain (1914)
Teaspoon Forged from a Silver Bar (Payne 1914)
A 6-inch silver teaspoon forged out of a small bar of silver, the way a blacksmith forges iron. Arthur Payne called it the hardest of his five spoon methods, but the cheapest, because almost no silver is wasted.
Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 184–186; annealing from his chapter XI. Cutting the bar from sheet is ours. Picture: Payne's Fig. 158, teaspoons forged this way.
Nâng cao
1 day
Hướng dẫn
1
1
Cut the silver bar
Cut the silver bar
For a teaspoon 6 in long you need a piece of sterling silver 4 in long, ½ in wide and ⅛ in thick. Mark it out and saw it from sheet of that thickness (cutting from sheet is ours).
Vật liệu cho bước này:
Tấm bạc sterling1 piece 4 × ½ × ⅛ inCông cụ cần thiết:
Mũi vạch dấu
Cưa thợ kim hoàn2
2
Forge out the bowl
Forge out the bowl
Heat the bar until it is almost red-hot, hold it in tongs and forge the bowl out on the anvil. Silver forges more easily when it is nearly red, but never hammer it while it is red-hot: it will crack.
Công cụ cần thiết:
Đèn Bunsen
Kẹp gắp
Đe
Búa3
3
Work bowl, then shank and handle
Work bowl, then shank and handle
Hammer the bowl until it is hard, then the shank and handle, so the whole spoon is hard before you anneal it again. That saves time.
Công cụ cần thiết:
Đe
Búa4
4
Anneal and repeat
Anneal and repeat
To soften it, heat it to a dull red and plunge it into water, or let it cool. Then go on forging until the spoon is roughly to shape.
Vật liệu cho bước này:
Nước1 as requiredCông cụ cần thiết:
Đèn Bunsen
Kẹp gắp
Bình thủy tinh5
5
Trim with shears and file
Trim with shears and file
Trim the outline with the shears and file the edges smooth.
Công cụ cần thiết:
Kéo cắt kim loại hạng nặng
Giũa (giũa tay)6
6
Polish out the file marks
Polish out the file marks
Rub out all the scratches and file marks with emery cloth.
Công cụ cần thiết:
Vải nhám emeri7
7
Anneal to even the fire scale
Anneal to even the fire scale
Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.
Vật liệu cho bước này:
Nước1 as requiredCông cụ cần thiết:
Đèn Bunsen
Kẹp gắp
Bình thủy tinh8
8
Planish with smooth hammers
Planish with smooth hammers
Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.
Công cụ cần thiết:
Búa là phẳng
Đe
Cọc9
9
Final polish with rouge
Final polish with rouge
Polish it lightly with a soft cotton flannel and a little red rouge.
Công cụ cần thiết:
Khăn đánh bóng trang sức
Bột đánh bóng đỏ của thợ kim hoànCông cụ yêu cầu
14- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.