Epoxy Resin
Pierre Castan, a Swiss chemist at the dental firm De Trey Frères, was looking for a resin for dentures. He reacted a phenol carrying two hydroxy groups with epichlorohydrin, then hardened the product with an acid anhydride, and got a hard, clear, unusually adherent solid. Ciba licensed it and sold it as Araldite; in the US Sylvan Greenlee developed epoxies independently.
**US 2,324,483**, "Process of preparing synthetic resins", Castan, granted 20. July 1943, claims condensing "a polybasic carboxylic acid anhydride" with the product of "a phenol having at least two phenolic hydroxy groups and of an epichlorhydrine". It does not single out bisphenol A, the phenol most epoxies use today.
**Epichlorohydrin is a carcinogen; you start from a two-part kit.** You glue pine lap joints at the right ratio and four wrong ones, then test hardness and break the joints.
Iniciante
2 hours plus 24 h cure
Instruções
1
1
Cut the joint pieces
Cut the joint pieces
Saw ten pine strips 100 x 25 mm. Sand one face of each end with 120 grit and dust off. Label five pairs 1:1, 1.25:1, 1:1.25, 1.5:1 and 1:1.5.
Materiais para este passo:
Tábua de pinho1 peça
Lixa1 folha
Fita de máscara1 roloFerramentas necessárias:
Serrote
Régua de aço
Lápis2
2
Measure by syringe
Measure by syringe
Gloves on. For each ratio draw resin and hardener in separate syringes (1:1 = 2 ml + 2 ml; 1.25:1 = 2.5 + 2; and so on) into its own cup. This assumes a 1:1-by-volume kit - scale to your label.
Materiais para este passo:
Epóxi de dois componentes25 mlFerramentas necessárias:
Luvas de nitrilo
Conjunto de seringas
Copos graduados de mistura
Óculos de segurança transparentes3
3
Mix thoroughly
Mix thoroughly
Stir each cup 2 minutes, scraping the walls and bottom. Unmixed streaks behave like a wrong ratio.
Ferramentas necessárias:
Vareta de agitação4
4
Glue and pour
Glue and pour
Spread each mix on the sanded ends of its pair, overlap them 25 mm and spring-clamp over wax paper. Pour the rest as a coin-sized puddle on wax paper beside it.
Materiais para este passo:
Papel encerado1 folhaFerramentas necessárias:
Grampo de mola5
5
Cure 24 hours
Cure 24 hours
Leave everything at room temperature, 20 °C or warmer, for 24 hours. Cold slows the cure.
6
6
Pencil hardness
Pencil hardness
Sharpen pencils 6B to 6H and flatten the tips on 400 grit. Push each at 45° across a puddle, from hard down, until one no longer scratches. Record that grade.
Ferramentas necessárias:
Jogo de lápis de grafite
Lupa de joalheiro7
7
Break the joints
Break the joints
Clamp one strip of a joint in the vise and tap the free end sideways with the mallet until it breaks. Estimate how much of the bond face is torn wood.
Ferramentas necessárias:
Torno de bancada
Maço de borracha
Óculos de segurança transparentes8
8
Ratio, leftovers, results
Ratio, leftovers, results
A carregar o notebook Jupyter…
9
9
History & Context
History & Context
**What the patent specifies:** a resin from a two-hydroxy phenol and epichlorohydrin, hardened by a polybasic acid anhydride. **Modern build (derived):** a two-part kit, most with an amine hardener that cures at room temperature.
Epoxy became the glue that holds metal, the matrix of fibreglass and carbon-fibre parts, and the boat-builder's resin. Its limits: it yellows in sunlight, softens with heat, and uncured resin and hardener sensitise skin - which is why the gloves stay on every time.
Materiais
5- 1 peçaReferência
- 1 folhaReferência
- 1 roloReferência
- Epóxi de dois componentes10% de comissão25 mlReferência
- 1 folhaReferência
Ferramentas necessárias
13- Referência
- Referência
- 1 vendor sell this, none ship to you yetReferência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
- Referência
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.