German Harness Leather: Limed, Bated and Bark-Tanned Hides Greased With Linseed Oil and Tallow (Davis, 1885)
Tex

Criado por

Tex

14. novembro 2026FO
7
0
0
0
0

German Harness Leather: Limed, Bated and Bark-Tanned Hides Greased With Linseed Oil and Tallow (Davis, 1885)

How German tanners made harness leather, from C. T. Davis's The Manufacture of Leather (1885): green hides soaked, limed twice, unhaired, fleshed and bated, tanned in old liquor and fresh tan with lay-aways until the cut is brown through, split into sides, smoothed, and greased on the flesh side with linseed oil and tallow; then sold brown or blacked with logwood and iron black.
Avançado
Several months

Instruções

1

His schedule

A carregar o notebook Jupyter…
2

Read The Manufacture of Leather, ch. XXXI

"Special attention should be paid to this process, as soft leather can only be produced by proper bating, while too much bating is injurious, as it destroys the skin fibres and the grain."
3

Soak and lime

Use green hides if possible. Cut out the horns, soak in running water 6 to 8 hours with frequent rinsing (not longer, or water-stripes form), clean off dung, and lay in weak milk of lime for 24 hours; take out, make fresh lime and replace for 24 hours more, then handle regularly. Salted hides need 3 days' soaking to remove all salt; dried hides are soaked and stretched back to shape.

Materiais para este passo:

Couro cruCouro cru1 peça
Cal apagadaCal apagada1 peça

Ferramentas necessárias:

Tina de curtimentaTina de curtimenta
Faca para couroFaca para couro
4

Unhair, flesh and bate

Unhair as soon as the hair pulls out easily, soak a few hours, flesh, soak 24 hours and smooth. Bate for 1 to 3 days by thickness and weather, handling three times a day; neither too little nor too much. Rinse, smooth again, soak several hours and work the flesh side thoroughly with a dull fleshing knife.

Ferramentas necessárias:

Cavalete de descarnarCavalete de descarnar
Faca de descarnarFaca de descarnar
Tina de curtimentaTina de curtimenta
5

Tan

Lay the hides in old liquor 1 or 2 days. Take them out, ladle out the old tan, add one third of a bushel of fresh tan and replace; the tan is spent in 4 to 8 days, so freshen the vat two or three times more. Then put them in the lay-aways, about as long as sole leather (stout harness leather may need longer). Split a hide after the second layer: uniformly brown through means tanned; pale yellow or white means not.

Materiais para este passo:

Casca de carvalho (triturada)Casca de carvalho (triturada)4 peças

Ferramentas necessárias:

Tina de curtimentaTina de curtimenta
Faca para couroFaca para couro
6

Split, smooth and grease

Split into sides and number both halves alike. Rinse in old ooze and smooth with a dull fleshing knife on the beam. Choose the best hides for harness. Go over the leather with a fine-edged knife, grease the flesh side with linseed oil and tallow, and hang it up to dry.

Materiais para este passo:

Óleo de linhaçaÓleo de linhaça1 peça
SeboSebo1 peça

Ferramentas necessárias:

Cavalete de descarnarCavalete de descarnar
Faca de descarnarFaca de descarnar
Faca para couroFaca para couro
Trincha largaTrincha larga
7

Finish brown or black

Sort into brown and black. Brown is sold as it is or given lustre by glassing. Black is grounded with a decoction of logwood, blacked with iron black and, when nearly dry, pressed.

Materiais para este passo:

Lascas de pau-campecheLascas de pau-campeche1 peça

Ferramentas necessárias:

Trincha largaTrincha larga
Panela grandePanela grande
8

Troubleshooting

Harness leather troubleshooting.

Flow

Loading...
9

History and honest limits

From Charles Thomas Davis, **The Manufacture of Leather** (Philadelphia, 1885), chapter XXXI (checked on the archive.org scan manufactureoflea01davi, pp. 518-521). He does not give the bate's composition, which tan, or the lime and oil-and-tallow quantities here; oak bark for the tan is our choice. The diagram hero and the tools are ours.

Materiais

6

Ferramentas necessárias

6

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.