Oak-Bark Calf-Skins: Lime, Dung Bate, Ooze and Two Three-Month Pits of Finest Tan (Morfit, 1852)
How calf-skins were tanned with oak bark, from Campbell Morfit's Arts of Tanning, Currying and Leather-Dressing (1852): limed in weakened vats, scraped, fleshed and beaten, bated in hen or pigeon dung, brought up in hot ooze and stronger ooze for a month, then laid folded in the finest tan in two pits of about three months each, ready for the currier.
Avançado
About 7 months
Instruções
1
1
Bark and weight
Bark and weight
A carregar o notebook Jupyter…
2
2
Read The Arts of Tanning, ch. XXVI
Read The Arts of Tanning, ch. XXVI
"The tanning of calf-skins is conducted much in the same way as that of small cow-hides."
3
3
Lime
Lime
Press the skins to expel the oily matter (dry skins are first trodden out and soaked). Pass them three times through old and once through fresh lime vats, using the vats after cow hides have weakened them, as calf cannot bear full-strength lime.
Materiais para este passo:
Pele de bezerro fresca12 peças
Cal apagada1 peçaFerramentas necessárias:
Tina de curtimenta4
4
Scrape, flesh and beat
Scrape, flesh and beat
Scrape off the lime, flesh carefully and rinse. Beat 15 to 18 skins in a tub for 8 to 10 minutes with wedge-shaped beaters 8-1/2 to 10 in high, after each rinsing (not needed where the skins are rinsed as often as six times).
Ferramentas necessárias:
Cavalete de descarnar
Faca de descarnar
Tina de curtimenta
Maço de madeira5
5
Bate
Bate
To clear the last lime, grease and glue, bate them in water with pigeon's or hen's dung, 10 to 12 gallons of dung to 100 skins, for 8 to 10 days, handling often and scraping on the beam, until they become pelts. (Fresh dung can putrefy and stain.)
Materiais para este passo:
Estrume animal1 peçaFerramentas necessárias:
Tina de curtimenta
Cavalete de descarnar
Faca de descarnar6
6
Ooze
Ooze
Put the pelts in hot ooze and water, handled more often and more carefully than cow hides, with fresh tan each time; then in stronger ooze and tan for a month.
Materiais para este passo:
Casca de carvalho (triturada)4 peçasFerramentas necessárias:
Tina de curtimenta7
7
Two pits
Two pits
Lay the skins in the pit folded lengthwise and unequally, spread with tan of the very finest quality, heads and tails (the thickest parts) with more; leave about 3 months. Take them out, clean off the tan, and lay them in a second pit of finest tan, folded the other way so the covered parts are now exposed; fill up, moisten with warm water (or warm bark infusion) and leave about 3 months. They are then ready for the currier.
Materiais para este passo:
Casca de carvalho (triturada)6 peçasFerramentas necessárias:
Tina de curtimenta8
8
Troubleshooting
Troubleshooting
Calf tanning troubleshooting.
Flow
Loading...
9
9
History and honest limits
History and honest limits
From Campbell Morfit, **The Arts of Tanning, Currying, and Leather-Dressing** (Philadelphia, 1852), chapter XXVI (checked on the archive.org scan artsoftanningcur00morf, pp. 349-353), with Kampffmeyer's oak-bark trial. He gives no ooze strengths. The diagram hero, the per-skin arithmetic and the tools are ours.
Materiais
4- 12 peçasReferência
- 1 peçaReferência
- 1 peçaReferência
- Referência
Este projeto faz
Blueprints relacionados
Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios
CC0 Domínio Público
Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.
Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.