Nylon Thread: Melt-Spun Monofilament, Cold-Drawn Between Two Drums, Carothers

Nylon sewing thread is a single clear strand, a monofilament. Carothers' patent (1938) spins nylon 66 straight from the melt at 285–295 °C, with oxygen kept out, and catches the strand on a drum. A second, faster drum then stretches it (cold drawing), which makes it strong. The picture: our own drawing.
Avançado
1 day

Instruções

1

Load the pot under nitrogen

Fill the melt-spinning pot with dry nylon 66 pellets and close it. Flush it with nitrogen and keep it under nitrogen: oxygen must stay out of the molten polymer.

Materiais para este passo:

Granulado de náilonGranulado de náilon500 g

Ferramentas necessárias:

Panela de fiação por fusãoPanela de fiação por fusão
AzotoAzoto
Garrafa de gás sob pressãoGarrafa de gás sob pressão
2

Melt at 285–295 °C

Heat to 285–295 °C, the best spinning heat for nylon 66. Cooler gives poorer filament; hotter makes it too runny, and it may break down.

Ferramentas necessárias:

Panela de fiação por fusãoPanela de fiação por fusão
Termopar com mostradorTermopar com mostrador
3

Extrude and catch it

Press the melt out through the hole with nitrogen pressure (Carothers' example used 50 lb/in²). Catch the strand on a motor-driven drum. A larger hole gives a thicker strand; hotter melt and faster winding give a finer one.

Ferramentas necessárias:

AzotoAzoto
Garrafa de gás sob pressãoGarrafa de gás sob pressão
Tambor de recolhimentoTambor de recolhimento
Motor elétricoMotor elétrico
4

Cold-draw onto a faster drum

Run the strand from the first drum onto a second drum turning faster, which stretches it. In Carothers' example the drums ran at 300 and 1020 ft/min. Keep the strand wet: wet filament draws better and holds no static.

Ferramentas necessárias:

Tambor de recolhimentoTambor de recolhimento
Motor elétricoMotor elétrico
ÁguaÁgua
5

Help a thick strand

Thick strands are harder to draw. Soak them in water, or warm them to about 100 °C, before drawing.

Ferramentas necessárias:

Tacho altoTacho alto
ÁguaÁgua

Materiais

1

Ferramentas necessárias

8

Blueprints relacionados

Estes blueprints compartilham conhecimento — técnicas, materiais ou princípios

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...