Reverberatory Furnace: the Air Furnace for Melting Cast Iron (Bolland, 1893)
Forge

Criado por

Forge

4. novembro 2026NO
13
0
0
0
0

Reverberatory Furnace: the Air Furnace for Melting Cast Iron (Bolland, 1893)

An air furnace melts iron apart from the fuel: coal burns on a grate at one end, and the flame is thrown down from a low arched roof onto the iron on the bed, then leaves by a tall chimney. The iron stays cleaner than in a cupola, so founders used it for guns, rolls, heavy scrap and lumps too big for the cupola. This furnace is 30 ft 6 in long and 7 ft wide outside, 5 ft wide inside, cased in bolted wrought-iron plates. Source: S. Bolland, The Iron Founder Supplement (1893), pp. 55-67. Unknown: brick sizes, plate thickness. Picture: Fig. 14 of the book.
Especialista
Unknown

Instruções

1

Lay the foundation

Build the foundation solid of common material up to the firebrick, shaped so the firebrick bed slopes down from the chimney end to the reservoir. Keep the bricks from B to C 6 in below the finished bottom, to leave room for the sand bed.

Materiais para este passo:

TijoloTijolo1 foundation

Ferramentas necessárias:

Colher de pedreiroColher de pedreiro
Dimensões desconhecidasDimensões desconhecidas
2

Build the fireplace, bridge and roof

Build the fireplace the full width of the furnace (5 ft inside, grate 5 ft long). Set the bridge wall at least 2 ft 3 in from the face of the grate bars. Build bridge, sides, roof and fireplace of the most refractory firebrick. Arch the roof the whole length, low, so it throws the flame down onto the bed; fill above the arches with common material. Leave the side charging hole (5 x 4 ft), the top hole (furnace width x 6 ft), the puddling hole over the reservoir, a sight hole and the tap hole.

Materiais para este passo:

Tijolos refratáriosTijolos refratários1 lining, bridge, roof
Argamassa de argila refratáriaArgamassa de argila refratária1 setting
TijoloTijolo1 filling above the arch
Metal desconhecidoMetal desconhecido1 grate bars

Ferramentas necessárias:

Colher de pedreiroColher de pedreiro
3

Case it in plates and bolt it

Case the whole structure in wrought-iron plates, held at the corners with angle-irons. Run eight chief anchor bolts from side to side, clear of all working parts. Join everything with bolts, not rivets, so any plate can come off for repairs. Line the charging doors with firebrick.

Materiais para este passo:

Placa de ferroPlaca de ferro1 casing, doors
Vergalhão de ferro forjadoVergalhão de ferro forjado8 anchor bolts
Metal desconhecidoMetal desconhecido1 angle-irons, door frames
Tijolos refratáriosTijolos refratários1 door linings

Ferramentas necessárias:

Dimensões desconhecidasDimensões desconhecidas
4

Build the chimney

Build the chimney square, 30 to 40 ft high, with an inside course of firebrick (Fig. 14: 2 ft 6 in square inside). Make its area a little larger than the fireplace. Put a damper on top that can be worked from the bottom: it alone sets the draught. It can stand apart on a sole plate on four columns.

Materiais para este passo:

Tijolos refratáriosTijolos refratários1 inside course
TijoloTijolo1 chimney
Metal desconhecidoMetal desconhecido1 damper

Ferramentas necessárias:

Colher de pedreiroColher de pedreiro
5

Make the sand bottom

Make the bottom from B round the reservoir to C with 8 parts fire-sand to 1 of clay and 1 of ground coke. Fire it well for one to two hours before the first charge; it should last ten heats. Fill the tap hole with fire-sand and a little coal dust, which will not cake when hot.

Materiais para este passo:

AreiaAreia8 parts
ArgilaArgila1 part
Coque metalúrgicoCoque metalúrgico1 part, ground

Ferramentas necessárias:

Carvão betuminosoCarvão betuminoso
6

Charge and melt

Fire with soft, non-caking bituminous coal and keep a full grate; clinker quickly and leave no holes for cold air. Charge all the iron at the start: first layer of pigs lengthwise and a little apart, next layers across, open so the flame passes. Set heavy pieces on firebricks so the flame plays all round them. Through the puddling hole, dip test pieces and skim the iron clean. To blend two grades, thrust green saplings into the melt. Close the damper before tapping. Look the furnace over after every heat.

Ferramentas necessárias:

Carvão betuminosoCarvão betuminoso
Lingotes de ferro-gusaLingotes de ferro-gusa
Vara de madeira duraVara de madeira dura
Escumadeira perfuradaEscumadeira perfurada

Materiais

9

Ferramentas necessárias

6

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.