Steel Pipe: Butt-Welded Through a Bell, Sized, Threaded and Tested (National Tube Co., 1921)

Butt-weld steel pipe, 1/8 to 3 inches, as National Tube made it in 1921: hot skelp is pulled by tongs and a draw-bench chain through a bell a little larger than the finished pipe, which curls it into a tube and presses its edges together into a weld. The pipe is then rolled to size, straightened, cleaned, threaded and pressure-tested. Each length, 20 to 40 ft, is welded in one pull. Every pipe is tested inside at 700 to 800 lb per square inch. Source: National Tube Co., "National" Modern Welded Pipe (1921), pp. 41-47. Picture: drawing butt-weld pipe.
Avançado
Unknown

Instruções

1

Heat the skelp

Charge the skelp from the rear into a long welding furnace, a little longer than the skelp, with a narrow opening at each end, and bring it to welding heat.

Materiais para este passo:

Banda de aço para tubosBanda de aço para tubos1 one piece per length of pipe

Ferramentas necessárias:

Forno de soldarForno de soldar
2

Draw it through the bell

Grip the trimmed end with long-handled tongs and pull it through a die, or bell, slightly larger than the finished pipe. Hook the tongs to the travelling chain of the draw bench, which pulls the whole length (20 to 40 ft) through. The skelp is a little wider than the bell's inside circumference, so it curls into a tube and its edges butt squarely and weld. Some sizes go through two bells at one heat, the second slightly smaller.

Ferramentas necessárias:

Banco de estiragemBanco de estiragem
Tenaz de forjaTenaz de forja
Forno de soldarForno de soldar
3

For Double Extra Strong pipe

Thick skelp needs so great a pull that a strong bar is welded on its end as a 'bait' for the tongs. Draw it several times through bells of decreasing size, reheating between draws, so the seam is thoroughly welded.

Ferramentas necessárias:

Banco de estiragemBanco de estiragem
Tenaz de forjaTenaz de forja
Forno de soldarForno de soldar
4

Size and round

Pass the pipe through sizing rolls, which reduce it slightly, lengthen it and loosen the heavy welding scale. Then roll it to its finished size and circular shape, which removes the scale and leaves the walls smooth.

Ferramentas necessárias:

LaminadorLaminador
5

Cool, straighten and clean

Let the pipe cool slowly as it crosses a table, then straighten and smooth it in cross rolls. Wash off the loosened scale in a tank; blow it out of the smaller sizes with compressed air.

Ferramentas necessárias:

LaminadorLaminador
ÁguaÁgua
Compressor de arCompressor de ar
6

Cut, thread and test

Cut off a short length at each end, where the tong jaws crushed it. Thread the pipe, then test it inside with water at 700 to 800 lb per square inch to prove the wall and the weld. Ours: hacksaw, die set and hand test pump; the booklet does not say how the ends are cut or threaded.

Ferramentas necessárias:

Serra de arco para metaisSerra de arco para metais
Jogo de machos e cossinetesJogo de machos e cossinetes
Bomba manual de ensaio de pressãoBomba manual de ensaio de pressão

Materiais

1

Ferramentas necessárias

9

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...