Silver Solder of Silver and Red Copper With a Burnt Wine-Stone Flux (Theophilus, 12th Century)
Forge

Criado por

Forge

14. novembro 2026NO
5
0
0
0
0

Silver Solder of Silver and Red Copper With a Burnt Wine-Stone Flux (Theophilus, 12th Century)

How Theophilus soldered silver in the 12th century: an alloy of two parts pure silver and a third part red copper, rasped to filings, laid on a joint painted with a flux of burnt wine-stone (tartar) ground with water and salt, and flowed in the coals with a long gentle blast.
Intermediário
About half a day

Instruções

1

The alloy

A carregar o notebook Jupyter…
2

Read De Diversis Artibus, Book III

"Weigh two parts of pure silver, and a third (part) of red copper, and mix and finely rasp into a clean vessel."
3

Make the solder

Weigh two parts of pure silver and a third part of red copper, melt them together, and rasp the alloy finely into a clean vessel; keep the filings in a quill.

Materiais para este passo:

Prata finaPrata fina1 peça
CobreCobre1 peça

Ferramentas necessárias:

Balança de pratosBalança de pratos
CadinhoCadinho
Tenaz para cadinhoTenaz para cadinho
Forja de ferreiroForja de ferreiro
FoleFole
GrosaGrosa
Pena de escreverPena de escrever
4

Make the flux

Take wine-stone from a vessel in which good wine has stood a long time, tie pieces in a cloth and put it in the fire until no more vapour comes from it. When cool, blow off the cloth ash and grind the burnt stone in a copper vessel with a round mallet, mixing in water and salt until it is as thick as lees.

Materiais para este passo:

Sarro de pipa (tártaro bruto)Sarro de pipa (tártaro bruto)1 peça
Pano de algodãoPano de algodão1 peça
SalSal1 peça

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Balde de 20 litrosBalde de 20 litros
Maço de madeiraMaço de madeira
5

Solder

With a thin piece of wood paint the flux round the joint inside and out, shake the filed solder over it with a small iron, and dry it. Paint more flux on, more thickly than before, put the work in the fire, cover it with coals and blow gently with a long breath until the solder has melted. Take it out, let it cool slightly and wash it. If the joint is not firm, do it again. Then file and scrape it smooth.

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
FoleFole
Tenaz para cadinhoTenaz para cadinho
Limas (lima de mão)Limas (lima de mão)
6

Troubleshooting

Soldering troubleshooting.

Flow

Loading...
7

History and honest limits

From Theophilus, **De Diversis Artibus**, Book III, chapter XXXI, translated by Robert Hendrie (1847) (checked on the archive.org scan essayuponvarious00hend, pp. 241-243). "A third (part)" can be read two ways; both are shown. Melting the alloy before rasping, the tools and the diagram are ours.

Materiais

5

Ferramentas necessárias

10

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.