Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper

Bromide paper is paper coated with silver bromide in gelatin, the printing and enlarging paper of the darkroom. Thorpe (1913) gives a beginner's emulsion: gelatin swelled in potassium bromide solution, silver nitrate made clear with strong ammonia, the two joined under ruby light, ripened, set, washed, and spread on paper as on a glass plate. From the moment the silver goes in, work only by ruby light. Grain and ounce figures are Thorpe's; the gram conversions and the 10-sheet batch are ours. The picture: our own drawing.
Erfahren
4 days

Anweisungen

1

Swell the gelatin

Dissolve 185 grains (12.0 g) of potassium bromide in 5 oz (142 ml) of water. Cover 300 grains (19.4 g) of hard gelatin with it and stir until it softens and swells.

Materialien für diesen Schritt:

KaliumbromidKaliumbromid12 g
GelatinepulverGelatinepulver19.4 g

Benötigte Werkzeuge:

WasserWasser
BecherglasBecherglas
GlasrührstabGlasrührstab
BalkenwaageBalkenwaage
2

Dissolve the silver

Dissolve 231 grains (15.0 g) of silver nitrate in 5 oz (142 ml) of water with gentle heat in the water bath. Add strong ammonia (0.880) a little at a time, stirring, until the precipitate that first forms dissolves again.

Materialien für diesen Schritt:

SilbernitratSilbernitrat15 g

Benötigte Werkzeuge:

WasserWasser
Starke Ammoniaklösung (0,880)Starke Ammoniaklösung (0,880)
BecherglasBecherglas
GlasrührstabGlasrührstab
Großer Topf (unten, für das Wasserbad)Großer Topf (unten, für das Wasserbad)
3

Melt the gelatin, never above 35 °C

Stand both vessels in the pan of water, never above 35 °C, stirring, until the gelatin is perfectly liquid. Up to here ordinary light is fine.

Benötigte Werkzeuge:

Großer Topf (unten, für das Wasserbad)Großer Topf (unten, für das Wasserbad)
ThermometerThermometer
GlasrührstabGlasrührstab
4

Add the silver under ruby light

From now on, ruby light only. Pour the silver solution into the gelatin in a thin stream, stirring all the time. Rinse the silver beaker with about 1 oz (28 ml) of warm water into the emulsion.

Benötigte Werkzeuge:

Rubin-DunkelkammerlampeRubin-Dunkelkammerlampe
BecherglasBecherglas
GlasrührstabGlasrührstab
WasserWasser
5

Ripen

Leave the emulsion in the hot water for half to three-quarters of an hour.

Benötigte Werkzeuge:

Großer Topf (unten, für das Wasserbad)Großer Topf (unten, für das Wasserbad)
Rubin-DunkelkammerlampeRubin-Dunkelkammerlampe
6

Set in the dark

Pour it into a flat dish, put it in a light-tight box and let it set for at least 24 hours; two or three days is better.

Benötigte Werkzeuge:

Flache KeramikschalenFlache Keramikschalen
Lichtdichter KastenLichtdichter Kasten
7

Wash through canvas

Scrape the set jelly onto wet coarse canvas and tie it into a bag. Knead it under water so it squeezes through in threads. Pour off the water, cover with fresh, wait 5 minutes and pour off: six to eight times.

Benötigte Werkzeuge:

PfannenwenderPfannenwender
SegeltuchSegeltuch
SchnurSchnur
WasserWasser
Rubin-DunkelkammerlampeRubin-Dunkelkammerlampe
8

Drain and store

Turn the threads onto a strainer covered with a cloth and let the water drain. Rinse with methylated spirit and keep in a lidded jar until coating.

Benötigte Werkzeuge:

SiebSieb
MusselintuchMusselintuch
BrennspiritusBrennspiritus
Glasgefäße mit DeckelGlasgefäße mit Deckel
Rubin-DunkelkammerlampeRubin-Dunkelkammerlampe
9

Coat the paper

Melt the emulsion in the warm water bath. Lay a sheet of paper flat on a levelled glass slab. Pour emulsion on the middle to cover nearly half the sheet, and spread it to each end with a glass rod 2 inches wider than the sheet, held just off the surface.

Materialien für diesen Schritt:

PapierPapier10 Blätter

Benötigte Werkzeuge:

Großer Topf (unten, für das Wasserbad)Großer Topf (unten, für das Wasserbad)
GlasscheibeGlasscheibe
WasserwaageWasserwaage
GlasrührstabGlasrührstab
Rubin-DunkelkammerlampeRubin-Dunkelkammerlampe
10

Dry

When the coat has set, move the sheets to a rack in a drying box with a current of air. They dry in 12 to 48 hours. Keep them in the light-tight box.

Benötigte Werkzeuge:

TrockengestellTrockengestell
Lichtdichter KastenLichtdichter Kasten

Materialien

4

Benötigte Werkzeuge

20

Dieser Bauplan stellt her

CC0 Gemeinfrei

Dieser Blueprint ist unter CC0 veröffentlicht. Sie dürfen dieses Werk für jeden Zweck frei kopieren, ändern, verbreiten und verwenden, ohne um Erlaubnis zu fragen.

Unterstützen Sie den Maker, indem Sie Produkte über seinen Blueprint kaufen, wo er eine Maker-Provision von Anbietern festgelegt, verdient. Oder erstellen Sie eine neue Iteration dieses Blueprints und verbinden Sie ihn in Ihrem eigenen Blueprint, um Einnahmen zu teilen.

Diskussion

(0)

Anmelden um an der Diskussion teilzunehmen

Kommentare werden geladen...