Forged Centre Punches and Pin Punches: Point Hardened in Brine, Temper Run to Straw from the Stock (Griswold, Amateur Work, 1904)
Forge

Creado por

Forge

14. noviembre 2026NO
4
0
0
0
0

Forged Centre Punches and Pin Punches: Point Hardened in Brine, Temper Run to Straw from the Stock (Griswold, Amateur Work, 1904)

Robert Gibson Griswold's first tool-making lesson in Amateur Work (Boston, 1904): four centre punches from heavy to fine and nine pin, drift, offset and riveting punches, forged from carbon tool steel, finished with file and emery, then the point alone dipped in brine and the temper let run down from the hot stock to straw yellow.
Intermedio
A day for the set

Instrucciones

1

His sizes

Cargando el cuaderno de Jupyter…
2

Read Griswold

"The more work put into the steel at the working point the better will be its grade."
3

Forge the blanks

Forge carbon tool steel at no more than a bright red into the shapes of his fig. 2: a 3/8 in. chamfered head, a 2 1/2 in. body and a 1 1/2 in. taper. Heavy centre punch at least 5/8 in. across with a conical point about 3/8 in. at the base; lighter centre punches 3/8 and 1/4 in.; pin punches 1/2, 3/8 (square end), 5/16 and 1/4 in., plus parallel-ended, offset and round-ended ones.

Materiales para este paso:

Barra de acero de herramientasBarra de acero de herramientas1 pieza

Herramientas necesarias:

Fragua de herreroFragua de herrero
YunqueYunque
MartilloMartillo
Tenazas de herreroTenazas de herrero
4

Finish before hardening

Do all work except grinding the point now: file each punch to shape and finish it with emery cloth. Keep the striking head slightly rounded so it does not broom.

Materiales para este paso:

Tela de esmerilTela de esmeril1 pieza

Herramientas necesarias:

Limas (lima de mano)Limas (lima de mano)
5

Harden the point

Heat the point to a dull red and plunge only the point, about 1/2 in. (13 mm), into a brine bath.

Materiales para este paso:

Salmuera saturadaSalmuera saturada1 pieza

Herramientas necesarias:

Fragua de herreroFragua de herrero
Tenazas de herreroTenazas de herrero
CuboCubo
6

Run the temper

When the point is black, rub a bright spot with emery cloth on a flat stick and watch the heat from the stock colour it. At straw yellow (460 F) plunge the whole punch in water and keep it moving. If the stock has too little heat, lay it over the furnace to draw the colour.

Materiales para este paso:

AguaAgua1 pieza
Tela de esmerilTela de esmeril1 pieza

Herramientas necesarias:

CuboCubo
Fragua de herreroFragua de herrero
7

Grind the points

Grind the points to shape after hardening without letting the edge turn blue; if it blues, grind back to hard metal.

Herramientas necesarias:

Esmeril de bancoEsmeril de banco
8

Troubleshooting

Punch troubleshooting.

Flow

Loading...
9

History and honest limits

From Robert Gibson Griswold, "Tool Making for Amateurs" I, **Amateur Work** (Boston), vol. III (1903-04), pp. 273-275 and fig. 2 (checked on the archive.org scan amateurwork03bostrich). Metric figures and tools are ours.

Materiales

4

Herramientas requeridas

7

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...