Nylon 66 Pellets: Nylon Salt Polymerised in an Autoclave, Carothers 1938
Mary

Creado por

Mary

17. octubre 2026FI
8
0
0
0
0

Nylon 66 Pellets: Nylon Salt Polymerised in an Autoclave, Carothers 1938

Nylon salt heated to 288 °C under oxygen-free nitrogen gives off water and joins into long chains of nylon 66 (Carothers, du Pont, US 2,130,948, 1938: two moles of salt in a silver-lined autoclave). A pinch of extra adipic acid keeps the melt's viscosity steady. The polymer is then extruded and cut into pellets. The picture: our drawing of the autoclave and the pellet line.
Avanzado
A day

Instrucciones

1

Charge the autoclave

Put two moles of nylon salt (525 g) and 0.02 mole of adipic acid (2.9 g) in a two-litre silver-lined autoclave with a stainless stirrer and a reflux condenser leading to a receiver.

Materiales para este paso:

Sal de nailonSal de nailon525 g
Ácido adípicoÁcido adípico2.9 g

Herramientas necesarias:

Reactor a presiónReactor a presión
Serpentín condensadorSerpentín condensador
Báscula digital de cocinaBáscula digital de cocina
2

Drive out the air

Evacuate, fill with nitrogen, evacuate again, then apply 80 lb/in² of nitrogen. Use nitrogen free of oxygen; oxygen spoils the polymer.

Herramientas necesarias:

Bomba de vacíoBomba de vacío
NitrógenoNitrógeno
ManómetroManómetro
3

Heat to 288 °C

Start the stirrer and heat to 288 °C over 1.5 hours.

Herramientas necesarias:

Reactor a presiónReactor a presión
Termopar con indicadorTermopar con indicador
4

Let the water off

Bring the pressure down to atmospheric over half an hour and keep heating and stirring 2.5 hours. Then pull to 200 mm absolute for a few minutes.

Herramientas necesarias:

Reactor a presiónReactor a presión
Bomba de vacíoBomba de vacío
ManómetroManómetro
Termopar con indicadorTermopar con indicador
5

Cool and take out

Cool. The polymer comes out as a white solid cake that melts at about 263 °C.

Herramientas necesarias:

Reactor a presiónReactor a presión
6

Pelletise

Break up the cake (our step), melt it in the extruder, draw the strand and cut it into pellets.

Herramientas necesarias:

Extrusora de plásticoExtrusora de plástico
Matriz de extrusiónMatriz de extrusión
7

Grams and pressures

Cargando el cuaderno de Jupyter…

Materiales

2

Herramientas requeridas

9

CC0 Dominio público

Este Blueprint se publica bajo CC0. Eres libre de copiar, modificar, distribuir y usar este trabajo para cualquier propósito, sin pedir permiso.

Apoya al Maker comprando productos a través de su Blueprint, donde gana una Comisión del Maker establecida por los vendedores, o crea una nueva iteración de este Blueprint e inclúyela como conexión en tu propio Blueprint para compartir ingresos.

Discusión

(0)

Iniciar sesión para unirte a la discusión

Cargando comentarios...