Forged Centre Punches and Pin Punches: Point Hardened in Brine, Temper Run to Straw from the Stock (Griswold, Amateur Work, 1904)
Forge

Créé par

Forge

14. novembre 2026NO
11
0
0
0
0

Forged Centre Punches and Pin Punches: Point Hardened in Brine, Temper Run to Straw from the Stock (Griswold, Amateur Work, 1904)

Robert Gibson Griswold's first tool-making lesson in Amateur Work (Boston, 1904): four centre punches from heavy to fine and nine pin, drift, offset and riveting punches, forged from carbon tool steel, finished with file and emery, then the point alone dipped in brine and the temper let run down from the hot stock to straw yellow.
Intermédiaire
A day for the set

Consignes

1

His sizes

Chargement du notebook Jupyter…
2

Read Griswold

"The more work put into the steel at the working point the better will be its grade."
3

Forge the blanks

Forge carbon tool steel at no more than a bright red into the shapes of his fig. 2: a 3/8 in. chamfered head, a 2 1/2 in. body and a 1 1/2 in. taper. Heavy centre punch at least 5/8 in. across with a conical point about 3/8 in. at the base; lighter centre punches 3/8 and 1/4 in.; pin punches 1/2, 3/8 (square end), 5/16 and 1/4 in., plus parallel-ended, offset and round-ended ones.

Matériaux pour cette étape :

Barre d'acier à outilsBarre d'acier à outils1 pièce

Outils nécessaires :

Forge de forgeronForge de forgeron
EnclumeEnclume
MarteauMarteau
Pinces de forgeronPinces de forgeron
4

Finish before hardening

Do all work except grinding the point now: file each punch to shape and finish it with emery cloth. Keep the striking head slightly rounded so it does not broom.

Matériaux pour cette étape :

Toile émeriToile émeri1 pièce

Outils nécessaires :

Limes (lime à main)Limes (lime à main)
5

Harden the point

Heat the point to a dull red and plunge only the point, about 1/2 in. (13 mm), into a brine bath.

Matériaux pour cette étape :

Saumure saturéeSaumure saturée1 pièce

Outils nécessaires :

Forge de forgeronForge de forgeron
Pinces de forgeronPinces de forgeron
SeauSeau
6

Run the temper

When the point is black, rub a bright spot with emery cloth on a flat stick and watch the heat from the stock colour it. At straw yellow (460 F) plunge the whole punch in water and keep it moving. If the stock has too little heat, lay it over the furnace to draw the colour.

Matériaux pour cette étape :

EauEau1 pièce
Toile émeriToile émeri1 pièce

Outils nécessaires :

SeauSeau
Forge de forgeronForge de forgeron
7

Grind the points

Grind the points to shape after hardening without letting the edge turn blue; if it blues, grind back to hard metal.

Outils nécessaires :

Touret à meulerTouret à meuler
8

Troubleshooting

Punch troubleshooting.

Flow

Loading...
9

History and honest limits

From Robert Gibson Griswold, "Tool Making for Amateurs" I, **Amateur Work** (Boston), vol. III (1903-04), pp. 273-275 and fig. 2 (checked on the archive.org scan amateurwork03bostrich). Metric figures and tools are ours.

Matériaux

4

Outils requis

7

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.