Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)
Charlie

Créé par

Charlie

28. octobre 2026DE
0
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)

A strontium ferrite with 0.06 mol strontium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 23. Went's rod held 2,120 gauss with a coercive force of 1,950 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 24. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avancé
2 days

Consignes

1

Weigh the carbonates and iron oxide

Weigh 8.86 g strontium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol), 95.55 g ferric oxide (0.6 mol). The patent prints 81.86 g of strontium carbonate beside 0.06 mol. 0.06 mol is 8.86 g (ours, at 147.63 g per mol), the weight used here.

Matériaux pour cette étape :

Carbonate de strontiumCarbonate de strontium8.86 g
Carbonate de calcium (blanc de Meudon)Carbonate de calcium (blanc de Meudon)4.004 g
Oxyde ferriqueOxyde ferrique95.55 g

Outils nécessaires :

Balance à fléauBalance à fléau
Masque respiratoire P100Masque respiratoire P100
2

Mill with alcohol 4 hours, dry

As in Example 23: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Outils nécessaires :

Broyeur à boulets de ferBroyeur à boulets de fer
Éthanol de laboratoire, 95 %Éthanol de laboratoire, 95 %
Étuve de séchageÉtuve de séchage
3

Press at 1.5 t/cm²

Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Outils nécessaires :

Presse hydrauliquePresse hydraulique
Matrice de pressage de disquesMatrice de pressage de disques
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Outils nécessaires :

Four tubulaireFour tubulaire
Gants résistants à la chaleurGants résistants à la chaleur
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Outils nécessaires :

ÉlectroaimantÉlectroaimant
BoussoleBoussole

Matériaux

3

Outils requis

11

CC0 Domaine public

Ce blueprint est publié sous CC0. Vous êtes libre de copier, modifier, distribuer et utiliser ce travail pour tout usage, sans demander la permission.

Soutenez le Maker en achetant des produits via son Blueprint où il perçoit une Commission Maker définie par les Vendeurs, ou créez une nouvelle itération de ce Blueprint et incluez-le comme connexion dans votre propre Blueprint pour partager les revenus.

Commentaires

(0)

Se connecter pour participer à la discussion

Chargement des commentaires...