Tuyere Iron: a Slotted Grate Cast in Grey Iron
Forge

Creato da

Forge

18. ottobre 2026NO
8
0
0
0
0

Tuyere Iron: a Slotted Grate Cast in Grey Iron

The tuyere is the opening in the bottom of the forge fire through which the blast is blown. Bacon (1919): its openings must let the blast through easily while keeping cinders from dropping into the blast pipe, and there should be a way to open the pipe below and clear out the cinders that still get through. This one is a slotted grate over a socket for the blast pipe, cast in grey iron. The design and sizes are ours. The picture: our drawing.
Avanzato
2 days

Istruzioni

1

Make the pattern

From pine, make a pattern of a square plate about 15 cm across and 2 cm thick with four or five narrow slots, and a short round socket under its centre to take the blast pipe. Taper every side slightly so it draws from the sand.

Strumenti necessari:

Tavola di pinoTavola di pino
Sega da traforoSega da traforo
Serie di scalpelli da legnoSerie di scalpelli da legno
Colla da legnoColla da legno
Calibro digitale da 6 polliciCalibro digitale da 6 pollici
2

Ram the mould

Ram the pattern up in casting sand in the flask, draw it out, and cut a sprue and a runner to the cavity.

Strumenti necessari:

Sabbia da fonderiaSabbia da fonderia
Staffa di formaturaStaffa di formatura
Paletta a manoPaletta a mano
3

Melt the iron

Melting pig iron in the cupola and tapping it into the ladle.
4

Pour

Pour the molten grey iron from the ladle into the sprue in one steady stream until the mould is full; about 4 kg with the sprue (our estimate). Let it cool in the sand.

Materiali per questo passaggio:

Pani di ghisa greggiaPani di ghisa greggia4 kg

Strumenti necessari:

Siviera da fonderiaSiviera da fonderia
Staffa di formaturaStaffa di formatura
Guanti da saldatoreGuanti da saldatore
Grembiule di cuoioGrembiule di cuoio
Visiera protettivaVisiera protettiva
5

Clean up

Shake out the casting, cut off the sprue, grind the fins and brush off the sand. Check that every slot is clear.

Strumenti necessari:

Smerigliatrice angolareSmerigliatrice angolare
Set di spazzole metallicheSet di spazzole metalliche
Guanti da saldatoreGuanti da saldatore
Visiera protettivaVisiera protettiva
6

Set it in the forge

Set it in the hearth with the blast pipe in its socket and a way to open the pipe below for clearing cinders. Richardson's forge had its tuyere iron four inches below the hearth surface.

Strumenti necessari:

Calibro digitale da 6 polliciCalibro digitale da 6 pollici

Materiali

1

Strumenti richiesti

14

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...