Glaze Fit: Crazing, Shivering, and the Mismatch Behind Both
Clay

작성자

Clay

24. 9월 2026DK
33
0
0
0
0

Glaze Fit: Crazing, Shivering, and the Mismatch Behind Both

A glazed pot is two materials stuck together that shrink by different amounts as they cool. If the difference is small, the glaze ends up gently squeezed and the pot is stronger for it. If it is large, something has to give. CRAZING is the glaze cracking into a network of fine lines, because the glaze shrank MORE than the body and is being stretched. SHIVERING is the glaze flaking off in slivers, because it shrank LESS and is being crushed. They are the same problem with opposite signs. Crazing is often left deliberately, as a decorative crackle. Shivering never is: the flakes are glass, they come off in use, and on anything that holds food that is a genuine hazard rather than a flaw.
고급
3 hours

안내

1

Tell them apart, and know which way to move

CRAZING looks like a fine web of cracks across the glaze surface, often appearing days or weeks after firing as the body slowly takes up atmospheric moisture and expands. Run a finger over it and it is smooth; the cracks are in the glass, not the surface. SHIVERING shows as sharp slivers lifting or flaking away, usually at edges, rims and handles where the glaze wraps a curve. It often appears with an audible ping as the kiln cools. A crazed pot is not waterproof even if it looks it — liquid travels through the cracks into the porous body, which is why a crazed mug eventually smells. That is the practical reason to care beyond appearance.

이 단계의 재료:

투명 유약투명 유약1 개
바짝 마른 점토 그릇바짝 마른 점토 그릇1 개

필요한 도구:

가마(킬른)가마(킬른)
2

The numbers behind the mismatch

Jupyter 노트북 불러오는 중…

이 단계의 재료:

투명 유약투명 유약1 개
세라믹 유약세라믹 유약1 개

필요한 도구:

데스크톱 컴퓨터데스크톱 컴퓨터
가마(킬른)가마(킬른)
3

Thickness and edges, before any chemistry

Before changing a recipe, check the application. Glaze that is too thick shivers at edges long before a well-fitted glaze would, because an edge has glaze on two faces meeting at a corner and nothing to hold it. Wipe glaze thinner on rims, handles and any sharp arris. Rounding sharp edges slightly while the pot is leather-hard also helps a great deal, and costs one pass with a damp sponge. Most reported glaze-fit faults turn out to be application faults. Chemistry is the answer when the fault persists on properly applied glaze across several firings — which is the change-one-thing-at-a-time rule saving a lot of wasted effort.

이 단계의 재료:

투명 유약투명 유약1 개

필요한 도구:

스펀지스펀지
도예 도구 세트도예 도구 세트
디지털 캘리퍼스 6인치디지털 캘리퍼스 6인치
4

Keep test tiles, and label them

Fire test tiles of every glaze on every body you use, with one, two and three dips on the same tile, and keep them. A shelf of tiles answers questions that no amount of reading will. Mark each tile with the glaze and body before firing — scratched into the clay, not written on with a pen that burns away. An unlabelled test tile is a pretty object of no use whatever. Record the firing too: which kiln, what schedule, what cone it reached. A glaze is a result of a recipe AND a firing, and the same bucket in a different kiln is a different glaze.

이 단계의 재료:

투명 유약투명 유약1 개
저화도 도토저화도 도토1 kg

필요한 도구:

도예 도구 세트도예 도구 세트
가마(킬른)가마(킬른)

재료

4

필요 도구

5

CC0 퍼블릭 도메인

이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.

제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.

토론

(0)

로그인 하여 토론에 참여하세요

댓글 로딩 중...