Steel Files: Forged, Cut and Hardened
A file is a bar of high-carbon steel, about 1.0–1.25 % carbon, covered in rows of tiny chisel cuts. The blank is forged with a tang, annealed soft, ground flat, and the teeth are raised one by one with a chisel and hammer: each blow cuts a groove and lifts its edge into a tooth. A single-cut file has one row of parallel cuts, at 65–85° to the length; a double-cut file has a second row crossing the first, for general work the first at 40–45° and the second at 70–80°. The file is then hardened as hard as it will go by quenching it in cold brine, and is never tempered; only the tang is softened so it will not snap. Factories do the same steps by machine.
고급
2 days (annealing overnight)
안내
1
1
Forge the blank
Forge the blank
At a yellow heat, draw the high-carbon steel to the file's section and forge a narrow, pointed tang at one end.
이 단계의 재료:
고탄소강 빌릿0.5 kg필요한 도구:
대장간 화덕
모루
단조 망치
대장간 집게2
2
Anneal
Anneal
Heat the blank no hotter than a blood-red and let it cool very slowly, shut away from the air; factories leave blanks in closed boxes in the furnace for 24–36 hours. Cooled in open air it would harden again.
필요한 도구:
대장간 화덕3
3
Straighten and grind
Straighten and grind
Straighten the blank, grind off the scale and make the faces flat and even, or the teeth will not be uniform.
필요한 도구:
회전 숫돌4
4
Cut the teeth
Cut the teeth
Hold the chisel at an angle and strike it, then move it a small, regular distance and strike again; each blow raises one tooth. For a double cut, cut the first row (overcut), then a second row crossing it (upcut). To cut the other face, turn the file over on a pewter plate so the finished teeth are not crushed.
필요한 도구:
줄눈 새김 정
단조 망치
모루
퓨터 판5
5
Harden
Harden
Heat the file evenly to its hardening heat and plunge it into a bath of cold brine, which cools faster than water and leaves it harder. Do not temper it.
이 단계의 재료:
소금1 kg필요한 도구:
대장간 화덕
양동이
대장간 집게6
6
Soften the tang
Soften the tang
Reheat the tang alone so it is no longer glass-hard: a fully hard tang snaps when the handle is driven on. Clean and oil the file.
필요한 도구:
대장간 화덕
대장간 집게이 블루프린트로 만드는 것
관련 블루프린트
이 블루프린트들은 지식을 공유합니다 — 기술, 재료 또는 원리
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.