Chemical-Resistant Gloves: Butyl Latex over Natural Rubber on a Cotton Liner (Hart & Collyer, US 4,190,685, 1980)
Tex

Ṣẹ́dá nipasẹ̀

Tex

3. Oṣù Kọkànlá 2026FO
16
0
0
0
0

Chemical-Resistant Gloves: Butyl Latex over Natural Rubber on a Cotton Liner (Hart & Collyer, US 4,190,685, 1980)

Dipped rubber gloves built in layers on a knitted cotton liner: one coat of natural rubber, then five coats of butyl rubber, which lets very little liquid or vapour through. Each coat is dipped from latex on a porcelain hand form, and the whole glove is cured under steam and air pressure. Made in Canada to protect soldiers against chemical warfare agents; worn gloves showed no penetration in 24 hours of field use. Result: flexible, soft chemical-resistant gloves with a comfortable cotton lining. Source: J. A. Hart and J. C. Collyer, US 4,190,685 (1980), latex method. Unknown: sizes, the pigments. Picture: the patent drawing.
Ilọsíwájú
Unknown

Ìlànà

1

Sew the cotton liner

Cut knitted or interlock cotton fabric to a glove shape and sew it into a glove. It stretches both ways, soaks up sweat and makes the glove easy to put on and take off. Not given: sizes, the knit.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Aṣọ òwú híhun-abẹ́rẹ́Aṣọ òwú híhun-abẹ́rẹ́1 liner

Àwọn irinṣẹ́ tí a nílò:

Ìṣẹ́náÌṣẹ́ná
Ẹ̀rọ ìránṣọẸ̀rọ ìránṣọ
Ìwọ̀n tí a kò mọ̀Ìwọ̀n tí a kò mọ̀
2

Dip in coagulant

Pull the liner onto a porcelain hand form and flame it to smooth off the surface. Dip it in a 10 % solution of acetic acid in acetone, then turn the form for about 2½ minutes at 24 °C until it is dry. The coagulant sets the latex before it can soak through the cloth.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Acid acetic (glacial)Acid acetic (glacial)1 10 % in acetone
AcetoneAcetone1 solvent

Àwọn irinṣẹ́ tí a nílò:

Àwòṣe ìbọ̀wọ́Àwòṣe ìbọ̀wọ́
Ọ̀pá Iná PùróféènìỌ̀pá Iná Pùróféènì
3

Dip the natural rubber coat

Dip the liner into natural rubber latex (the patent uses LOTOL 1185) and leave it 5 seconds. Draw it out, turn it upside down and let it dry. Scrub the rubber film with an abrasive cleaner, a brush and water, and dry it again.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Látẹ́ẹ̀sì rọ́bà àdáyébáLátẹ́ẹ̀sì rọ́bà àdáyébá1 bath
Ohun ìfọ̀ oníhóróOhun ìfọ̀ oníhóró1 as needed

Àwọn irinṣẹ́ tí a nílò:

Àwòṣe ìbọ̀wọ́Àwòṣe ìbọ̀wọ́
Búrọ́ọ̀ṣì ìfọ̀Búrọ́ọ̀ṣì ìfọ̀
4

Mix the butyl latex bath

Mix, in parts by dry weight: butyl rubber latex 100, sulphur 3, zinc dibutyldithiocarbamate 4, zinc oxide 5, formaldehyde 0.1 as a preservative, a liquid dithiocarbamate curing accelerator 4 (Merac 255 in the patent), and 6.5 of pigments (olive drab in the patent). Not given: the pigments.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Omi rọ́bà bútílìOmi rọ́bà bútílì100 parts dry
Imí-ọjọ́Imí-ọjọ́3 parts
Síńkì dáibútílìdáitáyókábámétìSíńkì dáibútílìdáitáyókábámétì4 parts
Lulú Sínkì Ọ́ksídìLulú Sínkì Ọ́ksídì5 parts
Omi formaldehyde (formalin 37 %)Omi formaldehyde (formalin 37 %)0.1 parts formaldehyde
Ohun ìmúyára dáitáyókábámétì olómiOhun ìmúyára dáitáyókábámétì olómi4 parts
Ohun èlò tí a kò mọ̀Ohun èlò tí a kò mọ̀6.5 parts pigment

Àwọn irinṣẹ́ tí a nílò:

Ohun ìrúwéOhun ìrúwé
5

Dip five butyl coats

Dip the glove into the butyl latex and draw it out at 10 cm per minute. At once turn the form at about 8 rpm at 24 °C until the film has gelled, then dry it upside down in an oven at 66 °C for 1 hour. Wash, dip and dry again until there are five butyl coats; do not use the abrasive cleaner on the butyl film.

Àwọn irinṣẹ́ tí a nílò:

Àwòṣe ìbọ̀wọ́Àwòṣe ìbọ̀wọ́
Ààrò ìgbẹ̀Ààrò ìgbẹ̀
6

Cure and finish

Dry the glove at 66 °C for 1 hour. Cure it for 3 hours in a pressure vessel with 30 psi steam in the jacket (131 °C) and 26 psi air in the chamber. Strip the gloves from the forms while hot; when cool, trim them and wash them in soapy water.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

ỌṣẹỌṣẹ1 as needed

Àwọn irinṣẹ́ tí a nílò:

Autoclave orí tábìlìAutoclave orí tábìlì
Ìṣẹ́náÌṣẹ́ná

Àwọn ohun-èlò

13

Àwọn irinṣẹ́ tó nílò

9

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.