Silicone (Rochow Direct Process)

Silicones - chains of silicon and oxygen carrying methyl groups - were known from Frederic Kipping's laboratory work, but could only be made a few grams at a time. In 1940 Eugene Rochow at General Electric found a one-step route: pass methyl chloride over hot silicon with copper, and methylchlorosilanes come straight off. Richard Müller found the same reaction independently in Germany, which is why it is also called the Müller-Rochow process. It is how silicones are still made. **US 2,380,995**, "Preparation of organosilicon halides", Rochow, assigned to General Electric, granted 7. August 1945, claims "effecting reaction between silicon and a hydrocarbon halide" with a copper catalyst at 200–500 °C. **Methyl chloride and chlorosilanes are toxic and stay in the plant.** You use the product: a two-part silicone mould of glass marbles, then cast hot wax in it, again and again.
Olùbẹ̀rẹ̀
4 hours plus two cures

Ìlànà

1

Build the box

Cut foam board and hot-glue an open box 60 x 40 mm inside, 50 mm tall. Seal every inside seam with a bead of glue - silicone finds any gap.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Àwo Fóòmù Ṣíṣe ÀwòṣeÀwo Fóòmù Ṣíṣe Àwòṣe1 ewé

Àwọn irinṣẹ́ tí a nílò:

Ọ̀bẹ Iṣẹ́ Ọwọ́Ọ̀bẹ Iṣẹ́ Ọwọ́
Ìbọn ìlẹ̀mọ́ gbígbónáÌbọn ìlẹ̀mọ́ gbígbóná
Ìwọ̀n IrinÌwọ̀n Irin
2

Clay bed and keys

Press sulphur-free modelling clay 20 mm deep into the box. Push two 16 mm marbles exactly halfway in, 20 mm apart. Press four dimples in the clay with a pencil end: these are the registration keys.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Amọ̀ ìṣe àwòránAmọ̀ ìṣe àwòrán150 g
Bọ́ọ̀lù dígíBọ́ọ̀lù dígí2 ẹyọ

Àwọn irinṣẹ́ tí a nílò:

Òṣùwọ̀n Kálípà Díjítà Ìnṣì 6Òṣùwọ̀n Kálípà Díjítà Ìnṣì 6
3

Weigh and mix

Weigh part A and part B at the kit's stated ratio into a mixing cup (the notebook gives the mass). Stir 3 minutes, scraping sides and bottom.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Ìdìpọ̀ ṣíṣe àwòṣe siliconiÌdìpọ̀ ṣíṣe àwòṣe siliconi1 ohun èlò

Àwọn irinṣẹ́ tí a nílò:

Òṣùwọ̀n Díjítà PípéÒṣùwọ̀n Díjítà Pípé
Àwọn kọ́ọ̀bù ìdàpọ̀ onípínÀwọn kọ́ọ̀bù ìdàpọ̀ onípín
Ọ̀pá ÌrúwéỌ̀pá Ìrúwé
4

First pour

Pour in a thin stream from 30 cm into one corner, never onto the marbles, until 6 mm above them. Cure for the kit's time.

Àwọn irinṣẹ́ tí a nílò:

Àwọn kọ́ọ̀bù ìdàpọ̀ onípínÀwọn kọ́ọ̀bù ìdàpọ̀ onípín
5

Flip and release

Flip the box, peel away all clay and leave the marbles in the silicone. Brush a thin coat of petroleum jelly over the silicone face - silicone bonds to silicone.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

VaselineVaseline5 g
6

Second pour

Mix a second batch the same way and pour 6 mm above the marbles. Cure again.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Ìdìpọ̀ ṣíṣe àwòṣe siliconiÌdìpọ̀ ṣíṣe àwòṣe siliconi1 ohun èlò

Àwọn irinṣẹ́ tí a nílò:

Òṣùwọ̀n Díjítà PípéÒṣùwọ̀n Díjítà Pípé
Àwọn kọ́ọ̀bù ìdàpọ̀ onípínÀwọn kọ́ọ̀bù ìdàpọ̀ onípín
7

Open and cut sprues

Tear off the foam board, part the halves and pop out the marbles. With the craft knife cut a 5 mm cone from the top face into each cavity.

Àwọn irinṣẹ́ tí a nílò:

Ọ̀bẹ Iṣẹ́ Ọwọ́Ọ̀bẹ Iṣẹ́ Ọwọ́
8

Cast wax

Melt paraffin wax in the double boiler to 75 °C. Band the halves shut, pour through each sprue, cool 30 minutes, open. Count how many casts it survives.

Àwọn ohun èlò fún ìgbésẹ̀ yìí:

Ìdí parafíìnìÌdí parafíìnì100 g
Okùn rọ́bàOkùn rọ́bà1 àkópọ̀

Àwọn irinṣẹ́ tí a nílò:

Ìkòkò méjì onímí omiÌkòkò méjì onímí omi
Ohun ìwọ̀n-ooru àdídùnOhun ìwọ̀n-ooru àdídùn
Ìbọ̀wọ́ wẹ́lídìnÌbọ̀wọ́ wẹ́lídìn
Gílásì Ààbò Tí Ó Mọ́Gílásì Ààbò Tí Ó Mọ́
9

Troubleshoot the mould

Work down in order; each question points to one step to redo.

Flow

Loading...
10

Reaction, pour size, siblings

Ń ṣí ìwé Jupyter…
11

History & Context

**What the patent specifies:** silicon reacted with a hydrocarbon halide over copper at 200–500 °C to give organosilicon halides. **Modern build (derived):** a two-part room-temperature-curing mould silicone. Silicone first served in the Second World War as grease and insulation for aircraft ignition systems; today it is sealant, bakeware, medical tubing and every maker's mould rubber. Its limits: it tears easily once nicked, is expensive, and a platinum-cure grade will not set against sulphur, some clays and latex gloves.

Àwọn ohun-èlò

7

Àwọn irinṣẹ́ tó nílò

11

CC0 Àgbègbè Gbogbogbò

Blueprint yìí ti jáde lábẹ́ CC0. O lè ṣe àdàkọ, yí padà, pín, àti lò láìsí ìyọ̀ǹda.

Ṣàtìlẹ́yìn Olùṣẹ́dá nípa rírà àwọn ọjà nipasẹ̀ Blueprint wọn Ẹ̀san Olùṣẹ́dá tí àwọn Olùtajà gbé kalẹ̀, tàbí ṣẹ̀dá àtúnṣe tuntun ti Blueprint yìí kí o sì fi sínú Blueprint rẹ gẹ́gẹ́ bí ìsopọ̀ láti pín owó-wíwọlé.

Ìfọ̀rọ̀wérọ̀

(0)

Wọlé láti dara pọ̀ mọ́ ìfọ̀rọ̀wérọ̀

Ń gbé àwọn ọ̀rọ̀ wọlé...