Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1240 °C (Went, Philips 1956, Ex. 29)
A ceramic magnet with both barium and strontium: 0.5 mol barium carbonate and 0.5 mol strontium carbonate to 2.5 mol iron oxide, milled as in Example 28, pressed and passed through a 1240 °C furnace in 10 minutes. Went's rod held 1,550 gauss with a coercive force of 3,410 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 29. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days
निर्देशनहरू
1
1
Weigh the carbonates and iron oxide
Weigh the carbonates and iron oxide
Weigh 99.2 g barium carbonate (0.5 mol), 73.8 g strontium carbonate (0.5 mol), 402.0 g ferric oxide (2.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
यस चरणका सामग्री:
ब्यारियम कार्बोनेट (विथराइट)99.2 ग्राम
स्ट्रन्सियम कार्बोनेट73.8 ग्राम
फेरिक अक्साइड402 ग्रामचाहिने औजार:
समभुज तराजु
रबरका पन्जा
P100 स्वास रक्षक2
2
Mill with alcohol 15 hours, dry
Mill with alcohol 15 hours, dry
As in Example 28: grind the mixture with alcohol in a ball mill for 15 hours, then dry it.
चाहिने औजार:
फलामे बल मिल
इथानोल - प्रयोगशाला श्रेणी, 95 %
सुकाउने भट्टी3
3
Press the powder
Press the powder
Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.
चाहिने औजार:
हाइड्रोलिक प्रेस
डिस्क थिच्ने डाइ4
4
Pass through a 1240 °C zone in 10 minutes
Pass through a 1240 °C zone in 10 minutes
Sinter at 1240 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
चाहिने औजार:
ट्युब फर्नेस
ताप सहने पन्जा5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
चाहिने औजार:
विद्युत् चुम्बक
दिशासूचक यन्त्रसामग्री
3- 99.2 ग्रामप्लेसहोल्डर
- 73.8 ग्रामप्लेसहोल्डर
- 402 ग्रामप्लेसहोल्डर
आवश्यक उपकरणहरू
12- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यो खाकाले बनाउँछ
सम्बन्धित ब्लुप्रिन्ट
यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त
CC0 सार्वजनिक डोमेन
यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।
ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।