Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)
Charlie

सिर्जनाकर्ता

Charlie

28. अक्टोबर 2026DE
२
०
०
०
०

Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)

A ceramic magnet with both barium and strontium: 0.09 mol barium carbonate and 0.21 mol strontium carbonate to 2.7 mol iron oxide, milled as in Example 28, pressed and passed through a 1300 °C furnace in 10 minutes. Went's rod held 1,340 gauss with a coercive force of 2,640 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 31. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days

निर्देशनहरू

1

Weigh the carbonates and iron oxide

Weigh 17.9 g barium carbonate (0.09 mol), 31.0 g strontium carbonate (0.21 mol), 435.5 g ferric oxide (2.7 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

यस चरणका सामग्री:

ब्यारियम कार्बोनेट (विथराइट)ब्यारियम कार्बोनेट (विथराइट)17.9 ग्राम
स्ट्रन्सियम कार्बोनेटस्ट्रन्सियम कार्बोनेट31 ग्राम
फेरिक अक्साइडफेरिक अक्साइड435.5 ग्राम

चाहिने औजार:

समभुज तराजुसमभुज तराजु
रबरका पन्जारबरका पन्जा
P100 स्वास रक्षकP100 स्वास रक्षक
2

Mill with alcohol 15 hours, dry

As in Example 28: grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

चाहिने औजार:

फलामे बल मिलफलामे बल मिल
इथानोल - प्रयोगशाला श्रेणी, 95 %इथानोल - प्रयोगशाला श्रेणी, 95 %
सुकाउने भट्टीसुकाउने भट्टी
3

Press the powder

Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.

चाहिने औजार:

हाइड्रोलिक प्रेसहाइड्रोलिक प्रेस
डिस्क थिच्ने डाइडिस्क थिच्ने डाइ
4

Pass through a 1300 °C zone in 10 minutes

Sinter in air at 1300 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

चाहिने औजार:

ट्युब फर्नेसट्युब फर्नेस
ताप सहने पन्जाताप सहने पन्जा
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

चाहिने औजार:

विद्युत् चुम्बकविद्युत् चुम्बक
दिशासूचक यन्त्रदिशासूचक यन्त्र

सामग्री

3

आवश्यक उपकरणहरू

12

सम्बन्धित ब्लुप्रिन्ट

यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त

CC0 सार्वजनिक डोमेन

यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।

ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।

छलफल

(0)

लग इन छलफलमा सामेल हुन

टिप्पणीहरू लोड गर्दै...