PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)
Charlie

सिर्जनाकर्ता

Charlie

28. अक्टोबर 2026DE
३
०
०
०
०

PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)

A PTFE dispersion is stable on the shelf, but stirred hard enough it curdles. Fifty seconds at 1000 rpm in a baffled beaker and the polymer floats up as a dry-looking, unwettable crumb. Washed and dried, it is a free-flowing powder for rolling into tape, or for cold lubricated extrusion. Source: J. F. Lontz (du Pont), US 2,593,583 (1952), Example 1. Lontz started from a dispersion made with disuccinic acid peroxide; ours is Berry's persulfate dispersion, diluted to his 17 %. Picture drawn by Youblob.
मध्यम
1 day

निर्देशनहरू

1

Dilute the dispersion to 17 %

Ours: stir the 34 % dispersion with an equal weight of distilled water to get 17 % solids, the strength Lontz used.

यस चरणका सामग्री:

PTFE को जलीय छरिएको घोलPTFE को जलीय छरिएको घोल1 part
आसुत पानीआसुत पानी1 part

चाहिने औजार:

समभुज तराजुसमभुज तराजु
बिर्को भएको सिसाको भाँडोबिर्को भएको सिसाको भाँडो
2

Set up the baffled beaker

A 1-gallon stainless beaker, 6.5 in across and 7.5 in deep, with four baffles about ⅜ × 1 in hanging from the cover to within 3 in of the bottom. Stirrer: open turbine, 4 blades 1½ in high, 5 in across, reaching to within 1 in of the bottom.

चाहिने औजार:

ब्याफलसहितको मथ्ने ट्याङ्कीब्याफलसहितको मथ्ने ट्याङ्की
चलाउने साधनचलाउने साधन
3

Stir hard at 176 °F for 50 seconds

Put in half a gallon of the 17 % dispersion and heat it to 176 °F (80 °C). Run the stirrer at 1000 rpm for 50 seconds (Lontz measured 0.72 hp per gallon). The polymer coagulates and floats, unwetted, on top.

चाहिने औजार:

ब्याफलसहितको मथ्ने ट्याङ्कीब्याफलसहितको मथ्ने ट्याङ्की
चलाउने साधनचलाउने साधन
तताउने प्लेटतताउने प्लेट
तापमापकतापमापक
4

Wash hot, then cold

Pour off the water. Wash the polymer with hot water at 176 °F, then with cold water at 60 °F (16 °C), and drain.

चाहिने औजार:

ब्याफलसहितको मथ्ने ट्याङ्कीब्याफलसहितको मथ्ने ट्याङ्की
तापमापकतापमापक
5

Dry at 230 °F for 16 hours

Spread the wet polymer on a 100-mesh screen and dry it in an oven at 230 °F (110 °C) for 16 hours. It comes out a free-flowing granular powder that passes 6–8 mesh.

चाहिने औजार:

मसिनो तार-जाली भएको चाल्नीमसिनो तार-जाली भएको चाल्नी
सुकाउने भट्टीसुकाउने भट्टी
बिर्को भएको सिसाको भाँडोबिर्को भएको सिसाको भाँडो

सामग्री

2

आवश्यक उपकरणहरू

8

सम्बन्धित ब्लुप्रिन्ट

यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त

CC0 सार्वजनिक डोमेन

यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।

ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।

छलफल

(0)

लग इन छलफलमा सामेल हुन

टिप्पणीहरू लोड गर्दै...