Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)
A strontium ferrite with a fifth of the strontium replaced by calcium: 0.08 mol strontium carbonate and 0.02 mol calcium carbonate to 0.6 mol iron oxide, ground, dried, formed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 2,320 gauss with a coercive force of 1,395 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 23. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days
निर्देशनहरू
1
1
Weigh the carbonates and iron oxide
Weigh the carbonates and iron oxide
Weigh 11.81 g strontium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol), 95.55 g ferric oxide (0.6 mol).
यस चरणका सामग्री:
स्ट्रन्सियम कार्बोनेट11.81 ग्राम
क्याल्सियम कार्बोनेट (सेतो खरी)2.002 ग्राम
फेरिक अक्साइड95.55 ग्रामचाहिने औजार:
समभुज तराजु
P100 स्वास रक्षक2
2
Mill with alcohol 4 hours, dry
Mill with alcohol 4 hours, dry
As in Examples 18 to 21: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.
चाहिने औजार:
फलामे बल मिल
इथानोल - प्रयोगशाला श्रेणी, 95 %
सुकाउने भट्टी3
3
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Example 23 does not say whether the 1000 °C presinter of Examples 18 to 21 is used. Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).
चाहिने औजार:
हाइड्रोलिक प्रेस
डिस्क थिच्ने डाइ4
4
Pass through a 1280 °C zone in 10 minutes
Pass through a 1280 °C zone in 10 minutes
Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
चाहिने औजार:
ट्युब फर्नेस
ताप सहने पन्जा5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
चाहिने औजार:
विद्युत् चुम्बक
दिशासूचक यन्त्रसामग्री
3- 11.81 ग्रामप्लेसहोल्डर
- 2.002 ग्रामप्लेसहोल्डर
- 95.55 ग्रामप्लेसहोल्डर
आवश्यक उपकरणहरू
11- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
- प्लेसहोल्डर
यो खाकाले बनाउँछ
सम्बन्धित ब्लुप्रिन्ट
यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त
CC0 सार्वजनिक डोमेन
यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।
ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।