Strontium Ferrite Disc Magnet: 0.7 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 12)
Charlie

सिर्जनाकर्ता

Charlie

28. अक्टोबर 2026DE
१
०
०
०
०

Strontium Ferrite Disc Magnet: 0.7 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 12)

A strontium ferrite: 0.7 mol strontium carbonate to 3.2 mol iron oxide, milled, bound and formed as in Example 4, and passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,955 gauss with a coercive force of 2,900 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 12. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
उन्नत
2 days

निर्देशनहरू

1

Weigh strontium carbonate and iron oxide

Weigh 103.3 g strontium carbonate (0.7 mol) and 503.0 g ferric oxide (3.2 mol).

यस चरणका सामग्री:

स्ट्रन्सियम कार्बोनेटस्ट्रन्सियम कार्बोनेट103.3 ग्राम
फेरिक अक्साइडफेरिक अक्साइड503 ग्राम

चाहिने औजार:

समभुज तराजुसमभुज तराजु
P100 स्वास रक्षकP100 स्वास रक्षक
2

Mill with alcohol 15.5 hours, dry and sieve

As in Example 4: grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

चाहिने औजार:

फलामे बल मिलफलामे बल मिल
इथानोल - प्रयोगशाला श्रेणी, 95 %इथानोल - प्रयोगशाला श्रेणी, 95 %
सुकाउने भट्टीसुकाउने भट्टी
चाल्नोचाल्नो
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

चाहिने औजार:

पोलिभिनाइल अल्कोहल धुलोपोलिभिनाइल अल्कोहल धुलो
हाइड्रोलिक प्रेसहाइड्रोलिक प्रेस
डिस्क थिच्ने डाइडिस्क थिच्ने डाइ
सुकाउने भट्टीसुकाउने भट्टी
4

Pass through a 1280 °C zone in 10 minutes

Sinter in air at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

चाहिने औजार:

ट्युब फर्नेसट्युब फर्नेस
ताप सहने पन्जाताप सहने पन्जा
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

चाहिने औजार:

विद्युत् चुम्बकविद्युत् चुम्बक
दिशासूचक यन्त्रदिशासूचक यन्त्र

सामग्री

2

आवश्यक उपकरणहरू

13

सम्बन्धित ब्लुप्रिन्ट

यी ब्लुप्रिन्टहरूले ज्ञान साझा गर्छन् — प्रविधि, सामग्री वा सिद्धान्त

CC0 सार्वजनिक डोमेन

यो ब्लुप्रिन्ट CC0 अन्तर्गत जारी गरिएको छ। तपाईं अनुमति नसोधी प्रतिलिपि, परिमार्जन, वितरण र प्रयोग गर्न सक्नुहुन्छ।

ब्लुप्रिन्ट मार्फत उत्पादनहरू किनेर सिर्जनाकर्तालाई सहयोग गर्नुहोस् सिर्जनाकर्ता कमिसन विक्रेताले तोकेको, वा यो ब्लुप्रिन्टको नयाँ संस्करण बनाउनुहोस् र आम्दानी बाँड्न आफ्नो ब्लुप्रिन्टमा जडानको रूपमा समावेश गर्नुहोस्।

छलफल

(0)

लग इन छलफलमा सामेल हुन

टिप्पणीहरू लोड गर्दै...