Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)
Forge

Nilikha ni

Forge

1. Nobyembre 2026NO
4
0
0
0
0

Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)

The renowned bar iron of Dannemora was refined in the old Walloon way: long white pigs melt drop by drop before a cold blast in a small, very hot charcoal hearth, the finer works the metal with an iron staff until it comes to nature, and the lump is drawn out under water-driven hammers. Result: bars 12 ft long of about 60 lb; 6 tons a week from one hearth, 80 % of the weight of the pig. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 599-601, after Tunner and A. Grill. Picture drawn by Youblob.
Dalubhasa
about 30 minutes per lump; 8-hour shifts

Mga Tagubilin

1

Build the finery hearth

Make the hearth of cast-iron plates: a 2-inch bottom plate on about 3 inches of pounded slag, over a cast-iron box with channels to drain water. From the tuyere it is 10-11½ inches to the back-plate, 22-24 inches to the work-plate and 22-24 inches to the opposite side. Depth: 7-8 inches under the tuyere, 14-15 under the back-plate, 15-18 opposite the tuyere. No tapping hole: the slag is never let out.

Mga kailangang kasangkapan:

Finery hearthFinery hearth
2

Set the tuyere and blast

The tuyere nozzle is semicircular, flat side down, 20-25 lines broad and 16-17 lines high, and projects 3½ inches; the blast-pipe nozzle sits 4 inches back inside it. Use cold blast. The blowing machine is not described.

Mga kailangang kasangkapan:

Finery hearthFinery hearth
Bulusan ng HanginBulusan ng Hangin
3

Lay in the pigs

Use white or strongly mottled pig in long pigs about 9 inches broad, 15-18 feet long, 3-4 inches thick at one end and 1-2 at the other. Lay them across the back-plate, one end sloping down over the tuyere, usually two one above the other, and push them forward as the ends melt.

Mga materyales para sa hakbang na ito:

Puting charcoal pig ironPuting charcoal pig iron1 long pigs

Mga kailangang kasangkapan:

Finery hearthFinery hearth
4

Light and make the slag bath

Fill the front of the hearth with moistened small charcoal and the rest with charcoal, light it and turn on the blast. To make enough slag bath, melt down some large finery scraps or, failing these, several shovelfuls of hammer scale.

Mga kailangang kasangkapan:

Uling - pinong durogUling - pinong durog
TubigTubig
UlingUling
Kaliskis ng bakalKaliskis ng bakal
PalaPala
5

Reheat the last bloom

At the start of each heat, hold the bloom from the last lump with tongs, as steeply as you can, in the front of the hearth to reheat it for drawing out.

Mga kailangang kasangkapan:

Sipit ng PandaySipit ng Panday
6

Work the metal with the staff

As soon as the first pig iron melts, work it with an iron staff: bring the metal on the tuyere side up from the bottom towards the middle into the blast, once to the left and once to the right of the reheating bloom. About 70 lb melts in 20 minutes; thin pieces of malleable iron then cling to the staff.

Mga kailangang kasangkapan:

Bilog na baras na bakalBilog na baras na bakal
7

Form the lump

Stop the flow of fresh molten pig, break up all the metal above the tuyere, melt it down and gather it into a lump about 12 by 15 inches. One lump takes 28 minutes on average (25-30).

Mga kailangang kasangkapan:

Bilog na baras na bakalBilog na baras na bakal
Sipit ng PandaySipit ng Panday
8

Draw out the bar

Heat each lump 6-8 times in a separate fire and draw it out under water-driven hammers into a bar 12 feet long of about 60 lb. One finery, one drawing-out forge and one hammer make 6 tons of bars a week; the bars weigh 80 % of the pig, and take 3 tons of charcoal per ton.

Mga kailangang kasangkapan:

PandayanPandayan
Martilyong ibinabagsakMartilyong ibinabagsak
Gulong-tubigGulong-tubig
Sipit ng PandaySipit ng Panday

Mga Materyales

1

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...