Steel Pipe: Butt-Welded Through a Bell, Sized, Threaded and Tested (National Tube Co., 1921)
Forge

Autor

Forge

4. listopad 2026NO
9
0
0
0
0

Steel Pipe: Butt-Welded Through a Bell, Sized, Threaded and Tested (National Tube Co., 1921)

Butt-weld steel pipe, 1/8 to 3 inches, as National Tube made it in 1921: hot skelp is pulled by tongs and a draw-bench chain through a bell a little larger than the finished pipe, which curls it into a tube and presses its edges together into a weld. The pipe is then rolled to size, straightened, cleaned, threaded and pressure-tested. Each length, 20 to 40 ft, is welded in one pull. Every pipe is tested inside at 700 to 800 lb per square inch. Source: National Tube Co., "National" Modern Welded Pipe (1921), pp. 41-47. Picture: drawing butt-weld pipe.
Zaawansowany
Unknown

Instrukcje

1

Heat the skelp

Charge the skelp from the rear into a long welding furnace, a little longer than the skelp, with a narrow opening at each end, and bring it to welding heat.

Materiały do tego kroku:

Taśma stalowa na ruryTaśma stalowa na rury1 one piece per length of pipe

Potrzebne narzędzia:

Piec do zgrzewaniaPiec do zgrzewania
2

Draw it through the bell

Grip the trimmed end with long-handled tongs and pull it through a die, or bell, slightly larger than the finished pipe. Hook the tongs to the travelling chain of the draw bench, which pulls the whole length (20 to 40 ft) through. The skelp is a little wider than the bell's inside circumference, so it curls into a tube and its edges butt squarely and weld. Some sizes go through two bells at one heat, the second slightly smaller.

Potrzebne narzędzia:

Ciągarka ławowaCiągarka ławowa
Kleszcze kowalskieKleszcze kowalskie
Piec do zgrzewaniaPiec do zgrzewania
3

For Double Extra Strong pipe

Thick skelp needs so great a pull that a strong bar is welded on its end as a 'bait' for the tongs. Draw it several times through bells of decreasing size, reheating between draws, so the seam is thoroughly welded.

Potrzebne narzędzia:

Ciągarka ławowaCiągarka ławowa
Kleszcze kowalskieKleszcze kowalskie
Piec do zgrzewaniaPiec do zgrzewania
4

Size and round

Pass the pipe through sizing rolls, which reduce it slightly, lengthen it and loosen the heavy welding scale. Then roll it to its finished size and circular shape, which removes the scale and leaves the walls smooth.

Potrzebne narzędzia:

WalcarkaWalcarka
5

Cool, straighten and clean

Let the pipe cool slowly as it crosses a table, then straighten and smooth it in cross rolls. Wash off the loosened scale in a tank; blow it out of the smaller sizes with compressed air.

Potrzebne narzędzia:

WalcarkaWalcarka
WodaWoda
Sprężarka powietrzaSprężarka powietrza
6

Cut, thread and test

Cut off a short length at each end, where the tong jaws crushed it. Thread the pipe, then test it inside with water at 700 to 800 lb per square inch to prove the wall and the weld. Ours: hacksaw, die set and hand test pump; the booklet does not say how the ends are cut or threaded.

Potrzebne narzędzia:

Piła do metaluPiła do metalu
Zestaw do gwintowaniaZestaw do gwintowania
Ręczna pompa próbna ciśnieniowaRęczna pompa próbna ciśnieniowa

Materiały

1

Wymagane narzędzia

9

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.