Rasps: Teeth Raised One at a Time with a Pointed Punch
Forge

Criado por

Forge

11. outubro 2026NO
33
0
0
0
0

Rasps: Teeth Raised One at a Time with a Pointed Punch

A rasp is a coarse file whose teeth stand separately instead of in continuous rows. Each tooth is raised by driving a pointed punch into the face of the blank at uniform distances. Because the teeth stand apart, a rasp clogs less than a cut file on soft material such as wood or a horse's hoof. The blank is forged, annealed and ground like a file blank, and the finished rasp is hardened like a file: coated against scale, brought to a dull red heat and plunged into water, with the tang tempered so it will not snap. Machine-made rasps have uniformly stamped teeth, which line up row behind row and leave deeper marks; slightly uneven hand-cut teeth avoid this.
Avançado
2 days (annealing overnight)

Instruções

1

Forge the blank

Forge the steel to a tapered bar, flat, round or half-round, with a narrow pointed tang at one end.

Materiais para este passo:

Lingote de aço de alto carbonoLingote de aço de alto carbono0.5 kg

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
BigornaBigorna
Martelo de forjaMartelo de forja
Tenaz de forjaTenaz de forja
2

Anneal and grind

Anneal the blank soft so the teeth can be raised, then grind the faces to a smooth, clear surface.

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
Mó de afiarMó de afiar
3

Punch the teeth

Drive the pointed punch into the face with the hammer at uniform distances, raising one separate tooth at each blow. Turn the rasp over on a soft metal plate to work the other face without crushing the finished teeth.

Ferramentas necessárias:

Punção de grosaPunção de grosa
Martelo de forjaMartelo de forja
BigornaBigorna
Placa de estanho (peltre)Placa de estanho (peltre)
4

Harden

Coat the toothed surface thickly with a salt composition against scaling, raise the rasp to a dull red heat in a clear coke fire and plunge it upright into water. If it bends, straighten it across a fulcrum before it is fully cold.

Materiais para este passo:

SalSal1 kg
Coque metalúrgicoCoque metalúrgico1 as required

Ferramentas necessárias:

Forja de ferreiroForja de ferreiro
BaldeBalde
Tenaz de forjaTenaz de forja
5

Temper the tang and clean

Temper the tang by dipping it in molten lead so it will not snap. Scour and wash off every trace of salt, then brush the rasp with oil.

Ferramentas necessárias:

Banho de chumbo fundidoBanho de chumbo fundido
Tenaz de forjaTenaz de forja

Materiais

3

Ferramentas necessárias

9

CC0 Domínio Público

Este blueprint é liberado sob CC0. Você é livre para copiar, modificar, distribuir e usar este trabalho para qualquer finalidade, sem pedir permissão.

Apoie o Maker comprando produtos através do Blueprint, onde ele ganha uma Comissão Maker definida pelos vendedores, ou crie uma nova versão deste Blueprint e inclua-o como conexão no seu próprio Blueprint para compartilhar receita.

Discussão

(0)

Entrar para participar da discussão

Carregando comentários...