Making Raw and Burnt Umber — The Manganese Earth Pigments of Warm Shadow and Deep Brown
Umber is a natural earth pigment composed of iron oxide and manganese dioxide mixed with clay and silica. The manganese content (5-20%) distinguishes it from other iron oxide earths like ochre and sienna — it gives umber its characteristic cool, greenish-brown tone and also makes it the fastest-drying earth pigment in oil (manganese accelerates oxidative polymerization of linseed oil). The name probably derives from Umbria in central Italy, though the finest historical sources were in Cyprus (where umber deposits are exceptionally rich in manganese).
Raw umber is a cool, dark brown with a greenish undertone. Burnt umber — produced by calcining raw umber at moderate temperatures — is a warm, reddish-dark brown, one of the most versatile and useful colours on any painter's palette. The calcination drives off chemically bound water from the goethite component, converting it to hematite, and partially oxidises the manganese dioxide, deepening and warming the colour dramatically. Both forms have been used continuously since antiquity in fresco, tempera, oil, and watercolour painting. They are completely lightfast, non-toxic, and compatible with every binder.
说明
Select and inspect raw umber earth
Select and inspect raw umber earth
Obtain raw umber earth from a geological supplier or art pigment dealer. Quality umber is a dark, cool brown with a distinctly greenish undertone when spread thin — this greenish cast is the hallmark of high manganese content. Rub a sample across white paper or an unglazed tile: the streak should be a cool grey-brown, not a warm reddish-brown (which would indicate low manganese, closer to a dark ochre). Cyprus umber is traditionally considered the finest quality. Remove any stones, roots, or organic debris.
此步骤所需材料:
Raw Umber Earth500 克Crush and grind to coarse powder
Crush and grind to coarse powder
Break the raw umber lumps into small fragments using a stone mortar and pestle. Pound and grind until the umber is a coarse, gritty powder with no pieces larger than a grain of rice. Wear a dust mask — umber dust is non-toxic but mineral dust should not be inhaled. Umber is typically softer and easier to crush than ochre because of its higher clay content, so this step goes quickly.
所需工具:
Stone Mortar and Pestle (large)
Dust MaskLevigate the raw umber
Levigate the raw umber
Place the crushed umber in a large glass settling jar and add water at approximately 5:1 ratio. Stir vigorously, then let stand for 30 seconds — the heavy sand and grit will settle immediately. Pour the cloudy brown suspension through muslin cloth into a second settling jar, discarding the coarse sediment. Let the second jar settle undisturbed for 4-6 hours, then carefully pour off the clear water above the settled pigment. Repeat if needed. The levigated raw umber should feel silky-smooth between the fingers with no grit.
所需工具:
Glass Settling Jar (5L)
Muslin Cloth
Stirring Rod (wooden)Dry and divide — reserve half as raw umber
Dry and divide — reserve half as raw umber
Spread the wet pigment paste on a clean glass surface and let it dry completely (1-2 days). Once dry, break the cake into pieces and grind half on a glass muller to a fine, smooth powder. This is your finished raw umber pigment — a cool, dark greenish-brown. Store in a sealed glass jar. Reserve the other half (as dried cake or coarse powder) for calcination in the next step.
所需工具:
Glass Muller
Clean Glass Jars with LidsCalcine to produce burnt umber
Calcine to produce burnt umber
Place the reserved raw umber in a clay crucible or refractory dish and heat in a kiln or over a strong fire. Bring the temperature gradually to 300-500°C and hold for 30-60 minutes. Watch the colour change: as the goethite converts to hematite and the manganese dioxide partially oxidises, the cool greenish-brown shifts to a rich, warm reddish-dark brown. The exact temperature determines the final shade — lower temperatures produce a more moderate warming, higher temperatures a deeper, more reddish tone. Do not exceed 600°C or the pigment may lose chroma and become dull. Let the crucible cool completely before handling.
所需工具:
Clay Crucible (refractory)
Crucible Tongs (long-handled)
Leather Gauntlet GlovesGrind the burnt umber to finished pigment
Grind the burnt umber to finished pigment
Once cooled, grind the calcined umber on a glass muller to a fine, smooth powder. Burnt umber should feel silky and produce a warm, rich reddish-brown when rubbed between the fingers. Compare it side by side with the raw umber from step 4 — the difference is dramatic: raw umber is cool and greenish, burnt umber is warm and reddish. Store in a sealed glass jar. Both pigments are permanent, completely lightfast, non-toxic, and compatible with all painting media. Burnt umber is especially valued in oil painting as an underpainting colour and for glazing warm shadows — the manganese content means it dries faster than any other earth pigment in oil.
所需工具:
Glass Muller
Clean Glass Jars with Lids材料
1- 500 克占位符
已连接蓝图材料
CC0 公共领域
此蓝图以 CC0 协议发布。你可以自由复制、修改、分发和使用此作品,无需征得许可。
通过购买蓝图中的产品支持创客,他们将获得 创客佣金 (由供应商设定),或创建此蓝图的新版本并将其作为连接包含在你自己的蓝图中以分享收入。