Making Raw and Burnt Umber — The Manganese Earth Pigments of Warm Shadow and Deep Brown
Umber is a natural earth pigment composed of iron oxide and manganese dioxide mixed with clay and silica. The manganese content (5-20%) distinguishes it from other iron oxide earths like ochre and sienna — it gives umber its characteristic cool, greenish-brown tone and also makes it the fastest-drying earth pigment in oil (manganese accelerates oxidative polymerization of linseed oil). The name probably derives from Umbria in central Italy, though the finest historical sources were in Cyprus (where umber deposits are exceptionally rich in manganese).
Raw umber is a cool, dark brown with a greenish undertone. Burnt umber — produced by calcining raw umber at moderate temperatures — is a warm, reddish-dark brown, one of the most versatile and useful colours on any painter's palette. The calcination drives off chemically bound water from the goethite component, converting it to hematite, and partially oxidises the manganese dioxide, deepening and warming the colour dramatically. Both forms have been used continuously since antiquity in fresco, tempera, oil, and watercolour painting. They are completely lightfast, non-toxic, and compatible with every binder.
안내
Select and inspect raw umber earth
Select and inspect raw umber earth
Obtain raw umber earth from a geological supplier or art pigment dealer. Quality umber is a dark, cool brown with a distinctly greenish undertone when spread thin — this greenish cast is the hallmark of high manganese content. Rub a sample across white paper or an unglazed tile: the streak should be a cool grey-brown, not a warm reddish-brown (which would indicate low manganese, closer to a dark ochre). Cyprus umber is traditionally considered the finest quality. Remove any stones, roots, or organic debris.
이 단계의 재료:
Raw Umber Earth500 gCrush and grind to coarse powder
Crush and grind to coarse powder
Break the raw umber lumps into small fragments using a stone mortar and pestle. Pound and grind until the umber is a coarse, gritty powder with no pieces larger than a grain of rice. Wear a dust mask — umber dust is non-toxic but mineral dust should not be inhaled. Umber is typically softer and easier to crush than ochre because of its higher clay content, so this step goes quickly.
필요한 도구:
Stone Mortar and Pestle (large)
Dust MaskLevigate the raw umber
Levigate the raw umber
Place the crushed umber in a large glass settling jar and add water at approximately 5:1 ratio. Stir vigorously, then let stand for 30 seconds — the heavy sand and grit will settle immediately. Pour the cloudy brown suspension through muslin cloth into a second settling jar, discarding the coarse sediment. Let the second jar settle undisturbed for 4-6 hours, then carefully pour off the clear water above the settled pigment. Repeat if needed. The levigated raw umber should feel silky-smooth between the fingers with no grit.
필요한 도구:
Glass Settling Jar (5L)
Muslin Cloth
Stirring Rod (wooden)Dry and divide — reserve half as raw umber
Dry and divide — reserve half as raw umber
Spread the wet pigment paste on a clean glass surface and let it dry completely (1-2 days). Once dry, break the cake into pieces and grind half on a glass muller to a fine, smooth powder. This is your finished raw umber pigment — a cool, dark greenish-brown. Store in a sealed glass jar. Reserve the other half (as dried cake or coarse powder) for calcination in the next step.
필요한 도구:
Glass Muller
Clean Glass Jars with LidsCalcine to produce burnt umber
Calcine to produce burnt umber
Place the reserved raw umber in a clay crucible or refractory dish and heat in a kiln or over a strong fire. Bring the temperature gradually to 300-500°C and hold for 30-60 minutes. Watch the colour change: as the goethite converts to hematite and the manganese dioxide partially oxidises, the cool greenish-brown shifts to a rich, warm reddish-dark brown. The exact temperature determines the final shade — lower temperatures produce a more moderate warming, higher temperatures a deeper, more reddish tone. Do not exceed 600°C or the pigment may lose chroma and become dull. Let the crucible cool completely before handling.
필요한 도구:
Clay Crucible (refractory)
Crucible Tongs (long-handled)
Leather Gauntlet GlovesGrind the burnt umber to finished pigment
Grind the burnt umber to finished pigment
Once cooled, grind the calcined umber on a glass muller to a fine, smooth powder. Burnt umber should feel silky and produce a warm, rich reddish-brown when rubbed between the fingers. Compare it side by side with the raw umber from step 4 — the difference is dramatic: raw umber is cool and greenish, burnt umber is warm and reddish. Store in a sealed glass jar. Both pigments are permanent, completely lightfast, non-toxic, and compatible with all painting media. Burnt umber is especially valued in oil painting as an underpainting colour and for glazing warm shadows — the manganese content means it dries faster than any other earth pigment in oil.
필요한 도구:
Glass Muller
Clean Glass Jars with Lids재료
1- 500 g플레이스홀더
필요 도구
10- 플레이스홀더
- 플레이스홀더
- 플레이스홀더
연결된 블루프린트 재료
CC0 퍼블릭 도메인
이 블루프린트는 CC0로 공개되었습니다. 어떤 목적으로든 자유롭게 복사, 수정, 배포 및 사용할 수 있습니다.
제품 구매를 통해 메이커를 지원하세요. 판매자가 설정한 메이커 커미션 을 받거나, 이 블루프린트의 새로운 반복을 만들어 연결로 포함시킬 수 있습니다.