Lead Ferrite Disc Magnet: 0.15 mol PbO2 to 0.9 mol Iron Oxide, Presintered at 900 °C (Went, Philips 1956, Ex. 17)
Mapanganib

Lead Ferrite Disc Magnet: 0.15 mol PbO2 to 0.9 mol Iron Oxide, Presintered at 900 °C (Went, Philips 1956, Ex. 17)

ni CharlieDE

Mga Materyales

8
0
0
0
0
0
Lead Ferrite Disc Magnet: 0.3 mol PbO2 to 1.5 mol Iron Oxide, Two-Stage Presinter (Went, Philips 1956, Ex. 16)
Mapanganib

Lead Ferrite Disc Magnet: 0.3 mol PbO2 to 1.5 mol Iron Oxide, Two-Stage Presinter (Went, Philips 1956, Ex. 16)

ni CharlieDE

Mga Materyales

9
0
0
0
0
0
Lead Ferrite Disc Magnet: 0.3 mol PbO2 to 1.2 mol Iron Oxide, Two-Stage Presinter (Went, Philips 1956, Ex. 15)
Mapanganib

Lead Ferrite Disc Magnet: 0.3 mol PbO2 to 1.2 mol Iron Oxide, Two-Stage Presinter (Went, Philips 1956, Ex. 15)

ni CharlieDE

Mga Materyales

5
0
0
0
0
0
Lead Dioxide: Red Lead Treated with Nitric Acid (Thorpe 1912)
Mapanganib

Lead Dioxide: Red Lead Treated with Nitric Acid (Thorpe 1912)

ni CharlieDE

Organiko

9
0
0
0
0
0
Barium Ferrite Disc Magnet from Natural Magnetite, Ground Half an Hour Only (Went, Philips 1956, Ex. 36, Procedure 3)

Barium Ferrite Disc Magnet from Natural Magnetite, Ground Half an Hour Only (Went, Philips 1956, Ex. 36, Procedure 3)

ni CharlieDE

Mga Materyales

9
0
0
0
0
0
Barium Ferrite Disc Magnet from Natural Magnetite, Pressed Without Presintering (Went, Philips 1956, Ex. 36, Procedure 2)

Barium Ferrite Disc Magnet from Natural Magnetite, Pressed Without Presintering (Went, Philips 1956, Ex. 36, Procedure 2)

ni CharlieDE

Mga Materyales

5
0
0
0
0
0
Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

ni CharlieDE

Mga Materyales

3
0
0
0
0
0
Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1300 °C (Went, Philips 1956, Ex. 34)

Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1300 °C (Went, Philips 1956, Ex. 34)

ni CharlieDE

Mga Materyales

7
0
0
0
0
0
Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)

Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)

ni CharlieDE

Mga Materyales

9
0
0
0
0
0
Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1100 °C (Went, Philips 1956, Ex. 34)

Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1100 °C (Went, Philips 1956, Ex. 34)

ni CharlieDE

Mga Materyales

6
0
0
0
0
0
Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)

Barium-Strontium Ferrite Disc Magnet: 0.09 mol BaCO3, 0.21 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 31)

ni CharlieDE

Mga Materyales

6
0
0
0
0
0
Barium-Strontium Ferrite Disc Magnet: 0.21 mol BaCO3, 0.09 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 30)

Barium-Strontium Ferrite Disc Magnet: 0.21 mol BaCO3, 0.09 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 30)

ni CharlieDE

Mga Materyales

6
0
0
0
0
0
Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1240 °C (Went, Philips 1956, Ex. 29)

Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1240 °C (Went, Philips 1956, Ex. 29)

ni CharlieDE

Mga Materyales

4
0
0
0
0
0
Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1260 °C (Went, Philips 1956, Ex. 28)

Barium-Strontium Ferrite Disc Magnet: 0.5 mol BaCO3, 0.5 mol SrCO3, 1260 °C (Went, Philips 1956, Ex. 28)

ni CharlieDE

Mga Materyales

2
0
0
0
0
0
Strontium-Calcium Ferrite Disc Magnet: Equal Strontium and Calcium, 1280 °C (Went, Philips 1956, Ex. 27)

Strontium-Calcium Ferrite Disc Magnet: Equal Strontium and Calcium, 1280 °C (Went, Philips 1956, Ex. 27)

ni CharlieDE

Mga Materyales

5
0
0
0
0
0
Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)

Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)

ni CharlieDE

Mga Materyales

3
0
0
0
0
0
Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)

Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)

ni CharlieDE

Mga Materyales

4
0
0
0
0
0
Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)

Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)

ni CharlieDE

Mga Materyales

8
0
0
0
0
0
Strontium Ferrite Disc Magnet: 0.6 mol SrCO3 to 3 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 13)

Strontium Ferrite Disc Magnet: 0.6 mol SrCO3 to 3 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 13)

ni CharlieDE

Mga Materyales

6
0
0
0
0
0
Strontium Ferrite Disc Magnet: 0.7 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 12)

Strontium Ferrite Disc Magnet: 0.7 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 12)

ni CharlieDE

Mga Materyales

7
0
0
0
0
0
Strontium Ferrite Disc Magnet: 0.8 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 11)

Strontium Ferrite Disc Magnet: 0.8 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 11)

ni CharlieDE

Mga Materyales

8
0
0
0
0
0
Strontium Ferrite Disc Magnet: 1 mol SrCO3 to 3 mol Iron Oxide, 1220 °C (Went, Philips 1956, Ex. 10)

Strontium Ferrite Disc Magnet: 1 mol SrCO3 to 3 mol Iron Oxide, 1220 °C (Went, Philips 1956, Ex. 10)

ni CharlieDE

Mga Materyales

8
0
0
0
0
0
Strontium Ferrite Disc Magnet: 1 mol SrCO3 to 2.5 mol Iron Oxide, 1200 °C (Went, Philips 1956, Ex. 9)

Strontium Ferrite Disc Magnet: 1 mol SrCO3 to 2.5 mol Iron Oxide, 1200 °C (Went, Philips 1956, Ex. 9)

ni CharlieDE

Mga Materyales

4
0
0
0
0
0
Strontium Ferrite Disc Magnet: Presintered at 1100 °C, 0.1 mol SrCO3 to 0.7 mol Iron Oxide (Went, Philips 1956, Ex. 8)

Strontium Ferrite Disc Magnet: Presintered at 1100 °C, 0.1 mol SrCO3 to 0.7 mol Iron Oxide (Went, Philips 1956, Ex. 8)

ni CharlieDE